1 Introduction
Cost-effectively making ethanol from cellulose is a national priority as well as a scientific challenge. With crude oil prices stubbornly stuck around $100/barrel, the world is now facing an energy crisis at a level that has never been seen before. Considering this fact, the U.S. Congress has passed the Energy Independence and Security Act of 2007 that mandates the production of 36 billion gallons of bioethanol, where 20 billion of those are from starch
(currently 9 billion) and 16 billion from cellulose (currently none) by 2022. Utilization of starch (mostly corn) as a source of ethanol has recently come into question because it competes with food supply, which led many to call starchbased ethanol a "devil's trade, food versus fuel". Hence, the focus is increasingly turning to cellulose (over one half of all global biomass) as the ultimate source for bioethanol [1].
Selective and effective separation of the main fractions present in lignocellulose biomass is of great interest, mainly when subsequently a submerged fermentation process will be performed, because the by-products obtained during hydrolysis of these materials may affect the fermentation yield and also because valuable sources are lost if other fractions are partially hydrolyzed. Since the structure of the plant cell wall components – cellulose, hemicelluloses and lignin – and the way they are linked with each other make it difficult to separate them, finding a suitable and effective separation process is quite a challenge. It can be in the form of biological, chemical, or physical processes, or a combination thereof. A number of effective mechanisms to perform the separation in view of facilitating the hydrolysis process of cellulose are given below.
The most frequent procedures to hydrolyze cellulose are chemical and enzymatic processes [2]. The chemical method, also known as concentrated acid hydrolysis, is conducted with mineral acids such as H2SO4 or HCl (in the range of 10~30%), at a temperature of about 160°C and a pressure of about 10 atm [3, 4]. The crystalline part of the cellulose makes this typical severe operation necessary in order to enable the cellulose to detach itself from its complex structure. However, this must be done warily so that by-products from the degradation of the important cellulose can be prevented. Hemicelluloses also need to be degraded with the presence of strong acids [2].
Moreover, corrosion issues can be avoided in the application of this method, while the advantage of minimum by-products and maximum whole glucose can be obtained, which is necessary for successful fermentation [2]. Enzymatic hydrolysis of cellulose is a reaction carried out by several cellulose-degrading enzymes: (1) endo-1,4-β-glucanase (EC 3.2.1.4), which attacks the amorphous regions of cellulose microfibrils; (2) exo-1,4-β-glucanases (EC 3.2.1.91, CBH as cellobiohydrolase), which attack their crystalline regions by removing cellobiose units either from the non-reducing ends or the reducing ends; (3) βglucosidase (EC 3.2.1.21), which hydrolyzes cellobiose to produce glucose [3- 6]. Many microbes, either bacteria or fungi, have been explored in order to find the most suitable one to be applied in enzymatic hydrolysis. One of these is Trichoderma reesei. However, T. reesei cellulases and their improvement
achieved by conventional techniques do not have adequate efficiency to make enzymatic cellulosic ethanol production economically viable at this time.
Due to the structural composition of lignocellulosic biomass, it has to go through a pretreatment process to make the cellulose easily penetrated during the enzymatic hydrolysis [2,7-9]. In this study, we applied simultaneous sacharification and fermentation (SSF) processes that have greater advantages compared to separate enzymatic hydrolysis and fermentation (SHF), since the inhibition effects of cellobiose and glucose to the enzyme are minimized by keeping a low concentration of these sugars in the media [10].
2 Materials and Methods
2.1 Ethanol Production
A piece of stem wood of S. uliginosa Foxw. was cut from a mature tree at a height of 2 to 3 m above the ground. The bark was peeled and the wood was airdried. The wood was then milled into a powder.
A mixture containing the powder of wood preparation (100 mg) in 2 ml of 50 mM sodium acetate buffer, pH 4.8, 0.02% Tween, 0.4 filter paper units of a cellulase preparation (2.0 mg) and a seed culture of Saccharomyces cervisiae (SH1089) with yeast nutrients (4 mg (NH4)2HPO4, 0.2 mg MgSO4.7H2O, and 8 mg yeast extract) was prepared. The mixture was incubated at 45°C in a rotary shaker set at 135 rpm. Each mixture was then subjected to simultaneous enzymatic saccharification and fermentation. About 100 µL of the supernatant was collected at 6 h, 12 h, 24 h, and 48 h of hydrolysis and then used for ethanol analysis. The ethanol formed was measured by gas chromatography on a Supelcowax-10 column (0.53 mm i.d. x 15 m; Supelco, Bellefonte, PA, USA) at 50°C using an Agilent gas chromatograph. Isopropanol was used as an internal standard.
2.2 Chemical Analysis
The wood powder was extracted 4 times successively with water and 24% KOH containing 0.1% NaBH4. The alkali-soluble fraction was neutralized, dialyzed, and freeze-dried for use in methylation analysis. Partially methylated alditol acetates were analyzed using an Agilent gas chromatography-mass spectrometer (Santa Clara, CA, USA) with a glass capillary column (0.25 x 15 m) of DB-225. Each alditol-acetate was identified by its retention time and mass spectrum. The amount of cellulose was determined by measuring the acid-insoluble residue; the samples were extracted with acetic/nitric reagent (80% acetic acid/concentrated nitric acid, 10:1) in a boiling water bath for 30 min. The resulting insoluble material was washed in water, air-dried and the amount of cellulose was measured. Lignin content was determined by the Klason method.
3 Results and Discussion
When saccharification was accompanied by fermentation with yeast, ethanol production was 22.0 mg/100 mg xylem in the enzymatic hydrolysate of the wood of S. uliginosa Foxw. The trend of ethanol production was similar to the trend of saccharification of the wood with cellulase preparation. The level of cellulose hydrolysis was almost complete at 48 h (Table 1). Based on chemical analyses, the level of cellulose in the wood of S. uliginosa Foxw. was 50.5% while its lignin content was 22.1%. The content of lignin in the wood was smaller than that of sengon (Paraserianthes falcataria), being 26.5% [11]. Based on methylation analysis of the hemicellulose fraction, the wood contained 0.1% of 4,6-linked glucose and 14.7% of 4-linked xylose, showing that the content of hemicelluloses (19.6%) was smaller than that of sengon (21.0%) [11].
Table 1 Saccharification and chemical components of S. uliginosa Foxw.
| Components | Persentage (%) |
|---|---|
| Saccharification 48 h | 52.6 |
| Cellulose | 50.5 |
| Lignin | 22.1 |
| Hemicellulose | 19.6 |
| 4-linked Xylose | 14.7 |
| 4,6-linked Glucose | 0.1 |
| Ash | 2.7 |
Our invention gives almost complete hydrolysis of lignocellulose of the wood of S. uliginosa Foxw., even though lignocellulose is believed to be recalcitrant to enzymatic saccharification. In addition, this invention provides a systematic method for using the wood of the S. uliginosa Foxw. tree as a lignocellulosic material for bioethanol production by saccharification and fermentation of xylem.
Low levels of xyloglucan and glucomannan along with a low lignin deposition in wood have been linked to the method for producing bioethanol from lignocellulose with an enzyme preparation. The surface of cellulose microfibrils may be less intercalated with xyloglucan. Therefore, our invention also shows that xyloglucan serves as a key hemicellulose and a tightening tether for the cellulose microfibrils in the secondary walls. The hydrolysis of the cellulose microfibrils by a cellulase preparation will have a higher rate if the amount of tether decreases in the wood. The level of recalcitrant compounds with regard to saccharification with cellulase enzyme preparation is lower compared to that of other trees. Therefore, there is no need for pretreatment of the wood before saccharification with fermentation.
Cellulase does not easily hydrolyze 1,4-β-glucans (cellulose microfibrils) intercalated with xyloglucan, nor does xyloglucanase efficiently attack xyloglucan in wood when the wood is subjected to saccharification with any commercial cellulase preparation. Xyloglucans intercalate tightly into cellulose microfibrils in wood because further elongation and expansion of the plant cells (fiber cells in wood) tighten and fix the intercalation between 1,4-β-glucan and xyloglucan during growth. Lignin is also bound to glucomannan, whose degradation could also reduce lignin deposition in the walls, because lignin is known to be a recalcitrant compound in cellulose hydrolysis.
Cellulose produced by plants is composed of both highly amorphous regions containing large voids and other irregularities, as well as a tightly packed crystalline region [12]. This region is frequently accepted as the reason behind the reactivity of a substrate [13]. The rate of cellulose hydrolysis mediated by fungal cellulases is typically 3-30 times faster for amorphous cellulose as compared to high crystalline cellulose [13]. Comparing the hydrolysis rates and the high level of crystalinty of S. uliginosa Foxw., it can be assumed that accessibility of cellulose is a more important factor in determining the hydrolysis rate than the crystallinity index.
4 Conclusions
The present invention relates to a method for producing bioethanol from lignocellulose of S. uliginosa Foxw. by saccharification and fermentation of its xylem. S. uliginosa Foxw. has a lower level of recalcitrant compounds with regard to saccharification with a cellulase enzyme preparation compared to other trees. Therefore, there is no need for pretreatment of the wood before saccharification with fermentation.