Nanucellulose from Tofu Production Waste for Wastewater Treatment

Abstract

Solid waste from tofu production, also known as okara, has numerous applications and can produce high-value-added products. However, the utilization of okara in Indonesia is not yet significant. This written work proposes okara as a source of nanocellulose to produce wastewater adsorbents in freshwater by fabricating it as aerogels and hydrogels. Wastewater is highly hazardous to the environment and living organisms as it can contain saturated salts, heavy metals, organic compounds, oil emulsions, dyes, and even microbes as pollutants that can lead to various diseases or death. Therefore, research on biosorbents is always a hot topic. Biosorption is the process of binding metal ions into the cellular structure of biological materials. Lignocellulosic biosorbents have high adsorption properties due to their ion exchange capability. Okara biosorbent can increase the absorption capacity of Pb2+ ions by up to 20% compared to conventional absorbents. The soybean skin component could also remove contaminated textile dyes from water. Additionally, the low lignin content in okara makes it easier to utilize than other lignocellulosic materials. This research study also shows that okara-based nanocellulose aerogels can maintain their shape or exhibit full shape recovery properties even after being used repeatedly.

Keywords

1 Introduction

Soy-based food products have become one of the primary sources of protein for the Indonesian population. In addition to the low cost of soy-based foods, soy also offers good nutritional value. It is well known that soy is one of the legumes with a high protein content. Just from the husk itself, soy contains 29-51% cellulose, 10-25% hemicellulose, 1-4% lignin, 4-8% pectin, 11-15% protein, and other extracts [1].

According to data from the Indonesian Ministry of Agriculture in 2013, tofu is the most consumed protein source by the Indonesian population. Tofu production itself reaches a minimum of 2.560.000 tons per year. However, it is not widely recognized that the tofu industry significantly contributes to waste. Research by

Diterima 27 November 2023, Direvisi 13 Desember 2023, Diterima untuk dipublikasikan 15 Desember 2023 Copyright ©2023 Diterbitkan oleh Fakultas Teknik Mesin dan Dirgantara ITB ISSN:0852-6095, DOI: 10.5614/MESIN.2023.29.2.2

Faisal et al. in 2016 revealed that small-scale tofu industries produce at least 20.000.000 m3 of liquid waste and 1.024.000 tons of solid waste annually. This waste equals 1.000.000 tons of CO2 gas emissions [2].

Solid and liquid waste from the tofu industry in Indonesia is still seldom utilized. Yet, tofu waste can be used for various high-value-added applications. Solid waste from tofu production, or okara, is commonly used as livestock feed due to its high protein content, and leaving okara exposed to open fields can produce unpleasant odors that pollute the environment. However, compared to other lignocellulosic materials, the application of okara is more versatile due to its extremely low lignin content (okara 1-4% [1], sugar cane bagasse 14-24% [3], and eucalyptus 27% [4]). Lignin is a major hindrance to the enzymatic hydrolysis of biomass [5]. Okara can also be processed into soil fertilizer [6] and food products.

One of the most fascinating applications of utilizing okara is one of the components in freshwater wastewater treatment. This benefit is undoubtedly exciting as wastewater issues are a global challenge that persists today. Wastewater is hazardous to the environment and living organisms due to its saturated salts, heavy metals, organic compounds, oil emulsions, dyes, and even microbes as pollutants that can cause various diseases. To address this issue, it is necessary to implement wastewater treatment for two primary purposes. Firstly, to efficiently recycle and reuse wastewater for human and other living organisms' consumption. The other is to guarantee adherence to environmental sustainability standards for wastewater discharge to minimize soil contamination [7].

Several methods can be employed to treat wastewater: chemically (chemical precipitation, oxidation, and reduction, electrochemical), mechanically (sedimentation, filtering), biologically (biofilters), or combination (coagulation, sorption, ion exchange, electrodialysis, reverse osmosis), etc. [8]. Additionally, adsorptions remain the most economical and efficient method as their concept and application are simple and flexible. Using biosorbents can efficiently remove both inorganic and organic pollutants [1].

Based on the previously explained issues, this review discusses the production of biosorbents by utilizing abundant waste in Indonesia, okara or soybean waste.

2 Composition of Okara

Soybean waste, known as okara, is a byproduct generally from the tofu and soymilk industry that generates tons worldwide annually. After curding and processing, every kilogram of soybean will produce 1.1-1.2 kg of fresh okara [6] that contains up to 84.5% moisture [9]. This review focuses on okara from the tofu industry, as shown in Figure 1. Okara contains up to 15.2-33.4% protein, 8.3-10.9% fat, 10.9% lipid, 3.8-5.3% low molecular weight carbohydrates, 42.4-58.1% dietary fiber including cellulose, hemicellulose, and lignin [9,10]. Other than that, every 100 grams of dry okara contains minerals, as listed in Table 1 [9,11.12].

TT 11 43.4"• . •C 1
Table 1Minerals coamnosition.of dryokara in mg.
Iabiciwillion and compositionor ar yokara m mg.
KNaCaMgFeMnZnCrP
935-
1350
16.2-
96
260-
428
130-
257
0.6-
8.2
0.2-
3.1
0.3-6.40.2396-
444

Okara reported having large amounts of hydroxyl and carboxyl groups in its components of cellulose and protein amino acids. This fact showed that okara is a good candidate for chemical modification, possibly being developed into biosorbent hydrogel and aerogel material [6]. These gel materials can be used for various applications such as soil supplements [6], tissue engineering, reduction of oil spills [13], and wastewater treatment [10,14].

Figure 1 Fresh okara from tofu production.

3 Biosorption using Okara Biosorbent

Biosorption refers to a metabolic-independent and passive process involving diverse interactions between a sorbate and a biological matrix called a biosorbent [15]. Biosorption is essential in numerous wastewater treatments. Evaluating the suitability of biosorbents is a crucial step in their selection. The use of biomass residue has gained significance for circular economic considerations. The environmentally friendly nature of biomass residue offers several benefits, addressing disposal concerns and providing economic advantages by generating revenue for various industries.

Many biomass residues can be used as biosorbents, including those based on cellulose [16], chitosan [17], algae [18], and okara [19]. The latter, okara-based biosorbents, are very interesting to develop, this biomass is very large in quantity, has functional groups that can bind heavy metal ions and organic pollutants, and is relatively easy to process, and can be used directly without further modification (Figure 2). Several types of pollutants that okara-based biosorbents can adsorb include heavy metal ions (Cd<sup>2+</sup>, Zn<sup>2+</sup>, Pb<sup>2+</sup>) [19,20], organic pollutants (methylene blue, safranin orange, reactive brilliant blue, brilliant green) [14] and anionic pollutants (PO<sub>4</sub><sup>3-</sup>) [21]. Another approach even utilized okara as it is without further modification, while others processed them to extract cellulose and nanocellulose content.

4 Preparation of Okara as Biosorbent

Some works have reported different approaches to fabricating okara-based biosorbents. Okara can be used as a biosorbent with or without further modification and functionalization (Figure 2). One of the advantages of okara is that it does not dissolve in water so that it can be separated after the adsorption process. To improve the performance of okara biosorbent, several studies reported modification and functionalization of okara, as seen in Table 2 and Table 3.

Hiew et al. [20] reported simple okara biosorbent preparation. Okara from industrial waste was rinsed and dried. The dried paste was blended to reduce it to smaller particles. The okara powder was then ground in an ultra-centrifugal mill and was screened through multiple sieves to obtain the biosorbent with particle sizes ranging from 125–200 µm. Nguyen et al. [21] reported okara biosorbents loaded with metal salt to activate their capability to capture phosphorous. In this work, fresh okara was treated with NaOH, followed with Fe (III) or (Zr(IV)). More than one metal can be incorporated into okara biosorbent. Yu et al. [22] loaded the surfactant onto okara to increase its adsorption capability towards methylene blue. okara was impregnated in sodium dodecyl sulfate, and then dried okara was powdered and sieved (<0.25 mm).

6

Figure 2 Okara utilization.

5 Heavy Metals Biosorption

Water contamination with heavy metals often comes from industries like battery manufacturing, metalwork, and plastic processing [23]. These heavy metals engage with active functional groups on the surface of the biosorbents. The biosorption mechanism includes the reduction of heavy metal ions, transforming them into less toxic forms. Table 2 shows several types of biosorbents and their capacity to bind heavy metals. Okara demonstrates moderate biosorption compared to other biomass biosorbents. It shows a biosorption capacity lower than rice husk, tomato waste, and pinecone but higher than banana peel and rice straw.

BiosorbentHeavy MetalBiosorption
Capacity (mg/g)
Reference
Banana PeelPb (II)0.5[24]
Cd (II)5.71[25]
Rice HuskCr (VI)33.68[26]
Tomato WastePb (II)152[27]
PineconePb (II)100.01
Cd (II)78.73
Cu (II)33.55[28]
Cr (VI)57.36
Rice StrawCd (II)3.77[29]
OkaraCd (II)14.80[20]
Zn (II)16.31[30]
Pb (II)11.13[30]

Table 2 Biosorbents from various types of biomass.

Several studies have indicated that okara can be used as a precursor for the removal of pollutants; for example, okara was used to remove Cd2+ [20], Zn2+ , and Pb2+ [19] from aqueous solution [30]. The Okara-metal biosorption may involve mechanisms, such as ionic exchange, hydrogen bonding, and electrostatic interactions [20].

The effects of contact time, solution pH, biosorbent dose, and initial solution concentration were studied. The results showed that the optimum was at Cd2+ solution pH 6.0 and Zn 2+ solution pH 7.0, with a solution concentration 50 mL. Okara biosorbent has an absorption capacity (q) of up to 14.80 mg/g of Cd2+ [20], 16.31 mg/g of Zn2+, and 11.13 mg/g of Pb2+ [30]. On the other hand, approximately okara has biosorption efficiency around 88.93-89.75% Cd2+ , 69.69-71.39% of Zn2+, and 95.18-99.91% of Pb2+ . The okara biosorbent also demonstrates regenerative capabilities. According to a study [20], despite a decrease in desorption efficiency from 89.21% to 32.56% after four cycles of regeneration using an HCl solution.

6 Organic Pollutant Biosorption

Okara is known to contain CHO, CO, and COOH functional groups on its surface, which are crucial in attracting different contaminants based on their surface charge. This property makes okara highly effective in eliminating heavy metals and organics such as azo dyes such as methyl orange, Eriochrome black-T, and rhodamine-B from textile industry effluents. Okara also has excellent removal capacity even at low pH (2.0), a distinct advantage compared to other biosorbents [14]. It has also been proven that okara effectively removes several organic pollutants with high adsorption capacity, as shown in Table 3. For example, Okara demonstrated adsorption of methylene blue up to 238.10 mg/g, while surfactant-modified okara increased the adsorption to 334.83 [22]. Okara also showed an adsorption capacity that reached 402.58 for Reactive Brilliant Blue KN-R.

Table 3 Okara biosorbent for organic pollutants.

NumOkara BiosorbentPollutantBiosorption
Capacity (mg/g)
Reference
1Okara and Sodium dodecyl sulfate activation okaraMethylene blue238.10 and 334.83[22]
2OkaraReactive Brilliant Blue
KN-R (RBB)
402.58[31]
3OkaraBrilliant green64.33[32]
4Okara modified with iron oxide nanoparticlesCyanotoxin2.84 μg/L[33]
5Acid treated okaraAcid Red 14 and
Reactive Red 15
217.39 and 243.90[34]
6OkaraMethylene Blue and
Safranin Orange
93.201 and
184. 592
[35]

7 Phosphorus Biosorption

Current research indicates the presence of phosphorus in okara, as shown in Table 1, suggesting a potential opportunity for phosphorus recovery from both okara and wastewater. Recognizing the limited capacity of untreated okara to remove

phosphorus from aqueous solutions, modified okara was created and employed for specific purposes. Raw okara exhibits a low q of 0.08 mg P/g. The previous study with iron load okara (ILO) demonstrated q of 16.39 mg phosphate/g. The presence of iron (Fe (II)) significantly improved phosphorus capture, facilitated by carboxymethylation that allowed the attachment of Fe (II). Zirconium and Iron/zirconium-loaded okara showed higher adsorption capacity than ILO, reaching 47.88 and 40.96 mg/g, respectively (Table 1) [21]. Compared to other metal-loaded biomass biosorbents, these adsorption values are relatively high.

Table 43-
Okara biosorbent in binding phosphorus(PO4
) [21].
NoOkara BiosorbentBiosorption
Capacity (mg/g)
1Iron loaded okara16.39
2Zirconium loaded okara47.88
3Iron/Zirconium loaded
okara
40.96

Phosphate adsorption by metal-loaded okara-based biosorbents likely occurs through the ligand exchange mechanism. This mechanism involves a process where there is an exchange between PO4 3 ions in the solution and OHions coordinated with the metal ions loaded on okara-based biosorbents. The loaded metal ions can easily transform into hydrated forms due to the abundant presence of OHions and H2O molecules. During hydrolysis, H2O molecules undergo deprotonation, releasing H+ ions to generate exchangeable OH- ions. These OHions can then be replaced by PO4 3 ions through the ligand exchange mechanism.

8 Okara Cellulose and Nanocellulose-based Biosorbent

As mentioned, okara contains a high amount of cellulose [10], a biopolymer composed of repeating β-1,4- glycoside-linked D-glucopyranose units [36]. Okara cellulose can be isolated via several processes; one example is shown in Fig. 3. Okara is treated by dispersing, drying, and washing several time to obtain its cellulose.

Okara can be used as nanocellulose precursors. The advantages of nanocellulosebased biosorbents include reduced adsorption time due to the nano-cellulose structure, low energy requirements for production, biodegradability, regeneration ability for reuse, and no generation of toxic sludge [1]. Nanocellulose is extracted from cellulose, resulting in less than 100 nm in size, as shown in Fig. 4 [37].

2

Figure 3 Isolation process of okara cellulose [36].

Nano-sized cellulose has significantly different properties compared to bulk cellulose. Nanocellulose is a sustainable nanomaterial with outstanding mechanical properties, biocompatibility, biodegradability, etc. The surface modification of nanocellulose can easily create new binding sites that provide specific characteristics for absorbing several types of pollutants. Surface modification of nanocellulose is emerging as a current and future research field in developing new biosorbents for environmental improvement [38].

Figure 4 Nanocellulose structures.

Nanocellulose can be prepared via various routes, such as acid and base hydrolysis. Besides that, nanocellulose can also be produced using ultrasonic homogenizer underwater bath conditions to obtain nanocellulose [39]. Research

conducted by Wu et al. in 2020 showed that ultrasonic and pressure homogenizers effectively disintegrate and disrupt thick cellulose fibers [36]. Nanocellulose that has undergone the sonication process is subsequently dried to obtain nanocellulose powder. Li et al. [40] prepared nanocellulose from okara to result in the form of nanofiber. They employed different mechanical homogenization, as shown in Fig. 6. It shows the formation of cellulose nanofiber with a diameter range of 5-45 nm.

3

Figure 5 Isolation of cellulose nanofiber from okara [40].

5

Figure 6 Morphology and diameter of okara cellulose nanofibers prepared by high-pressure homogenization (a, d), ultrasonic treatment (b, e), and high-speed stirring (c, f) [40].

In a study conducted by Cui et al. (2019) [10], FT-IR characterization was performed for samples of okara powder, okara cellulose, okara cellulose hydrogel, sigma cell cotton cellulose, and cotton cellulose hydrogel. All these samples exhibit the same absorption region at a wavenumber 3410 cm-1 , corresponding to the stretching of -CH3 groups, which are not found in the okara

cellulose sample. The peak at 1744 cm-1 in the okara sample suggests the presence of C=O groups, which are also absent in okara cellulose. Additionally, the peak at 1530 cm -1 corresponds to the stretching vibration of C-C bonds in aromatic rings, which is not found in the okara cellulose sample. These three peaks are associated with lipids, proteins, hemicellulose, and lignin in okara.

Okara nanocellulose powder obtained from the process can be formed into two biosorbents: aerogel and hydrogel. Aerogel and hydrogel compromise a solid three-dimensional network that forms the structure and a medium inside it, while the medium of aerogel is air and hydrogel is liquid [41]. Nanocellulose-based aerogels have attracted significant interest lately because of their remarkable adsorption capabilities, environmentally sustainable potential, and costeffectiveness.

The porosity of the fabricated nanocellulose hydrogels and aerogels is important. Pores in wastewater treatment have a role in adsorbing and absorbing pollutants into the gels and trapping them [42]. The porous nanocellulose aerogel base has been proven in the research conducted by Jiang and Hsieh in 2014 [43]. Fabricating okara nanocellulose biosorbents into aerogels or hydrogels will result in abundant advantages, as gels absorb vast amounts of liquids and contents. Other than that, nanocellulose gels-based biosorbents have high porosity, specific surfaces that can be adjusted according to our needs, high mechanical strength, low density, biodegradability, and hydrophilic [41].

Nanocellulose in gels has proven to have excellent adsorption capacity and increased effectiveness in binding compared to other biosorption materials due to the specific characteristics of nanocellulose, such as its high area specificity and the abundant amount of -OH groups present in its structure. These -OH groups contribute to binding pollutants and enable potential modification processes such as pollution remediation [44].

Ji et al. [45] reported that cellulose nanofiber aerogel efficiently captured diverse oils and organic solvents from water, demonstrating maximum absorption capacities reaching up to 108 g/g. Mo et al. [46] demonstrated that modified nanocellulose aerogel displays excellent absorption capability towards Cu (II), reaching an uptake capacity of 300 mg/g. Other research reported that biosorbents from other nanocellulose, such as hardwood kraft pulp and PVA aerogel, have the maximum capacity adsorption for Hg2+ (157.5 mg/g), Pb2+ (22 mg/g), Cu2+ (110.6 mg/g), and Ag2+ (24.5 mg/g) where these numbers were much higher than pure PVA aerogel [16].

Furthermore, okara showed cost-effectiveness as most of them were dumped and burned since there were no proper utilization techniques to process them. This abundant source is very effective for synthesizing value-added products, and since okara is considered a waste, the price will be lower than unprocessed soybeans [14]. Dumping and burning okara without any treatment can cause other problems, such as water and air pollution, since the waste contains a lot of organic substances [2].

9 Conclusion

Okara, the byproduct of tofu production, is potentially processed for various applications, including as a biosorbent in water through aerogels and hydrogels. Compared to other lignocellulosic materials, okara stands out due to its lower lignin content, enabling a quicker enzymatic hydrolysis cycle in obtaining cellulose. This ease of delignification makes okara versatile in applications. Okara-based gels potentially bind heavy metals and even other organic compounds produced by various industries. Repurposing soybean waste as a biosorbent adds value to agricultural residues and addresses environmental concerns, particularly in Indonesia, where okara waste is abundant.

10 References

  • [1] Liu, H.M. & Li, H.Y., Application and Conversion of Soybean Hulls, Soybean - The Basis of Yield, Biomass and Productivity, Minobu Kasai, Intech, pp. 111-132, 2017.
  • [2] Faisal, M., Gani, A., Mulana, F. & Daimon, H., Treatment and Utilization of Industrial Tofu Waste in Indonesia, Asian J. Chem., 28(3), pp. 501– 507, 2016.
  • [3] Mahmud, M.A. & Anannya, F.R., Sugarcane bagasse - A source of cellulosic fiber for diverse applications, Heliyon, 7(8), article number 07771, 2021.
  • [4] Chen, X., Zhang, K., Xiao, L.P., Sun, R.C. & Song, G., Total utilization of lignin and carbohydrates in Eucalyptus grandis: An integrated biorefinery strategy towards phenolics, levulinic acid, and furfural, Biotechnol Biofuels, 13(2), pp. 1–10, 2020.
  • [5] Chen, X., Li, H., Yao, S., Wang, C., Chen, X., Guo, H., Xiong, L., Zhang, H. & Chen, X., The alleviation of lignin inhibition on enzymatic hydrolysis of cellulose by changing its ultrastructure, Industrial Crop. Prod., 185, Article number 115108, 2022.
  • [6] Zhu, J., Tan, W.K., Song, X., Gao, Z., Wen, Y., Ong, C.N., Loh, C.S., Swarup, S. & Li, J., Converting Okara to Superabsorbent Hydrogels as Soil Supplements for Enhancing the Growth of Choy Sum (Brassica sp.) under Water-Limited Conditions, ACS Sustain. Chem. Eng., 8(25), pp. 9425–9433, 2020.

  • [7] Nishat, A., Yusuf, M., Qadir, A., Ezaier, Y., Vambol, V., Khan, M.I., Moussa, S. Ben, Kamyab, H., Sehgal, S.S., Prakash, C., Yang, H.-H., Ibrahim, H. & Eldin, S.M., Wastewater treatment: A short assessment on available techniques, Alexandria Eng. J., 76, pp. 505–516, 2023.
  • [8] Bryukhov, M. & Ulrikh, D., Wastewater treatment: Methods and prospects, IOP Conf. Ser. Earth Environ. Sci., 1061(1), article number 012049, 2022.
  • [9] Li, B., Qiao, M. & Lu, F., Composition, Nutrition, and Utilization of Okara (Soybean Residue), Food Rev. Int., 28(3), pp. 231–252, 2012.
  • [10] Cui, X., Lee, J.J.L. & Chen, W.N., Eco-friendly and biodegradable cellulose hydrogels produced from low cost okara: towards non-toxic flexible electronics, Sci. Rep., 9(1), pp. 1–9, 2019.
  • [11] van der Riet, W.B., Wight, A.W., Cilliers, J.J.L. & Datel, J.M., Food chemical investigation of tofu and its byproduct okara, Food Chem., 34(3), pp. 193–202, 1989.
  • [12] Mateos-Aparicio, I., Redondo-Cuenca, A., Villanueva-Suárez, M.J., Zapata-Revilla, M.A. & Tenorio-Sanz, M.D., Pea pod, broad bean pod and okara, potential sources of functional compounds, Lwt, 43(9), pp. 1467–1470, 2010.
  • [13] Arboleda, J.C., Hughes, M., Lucia, L.A., Laine, J., Ekman, K. & Rojas, O. J., Soy protein-nanocellulose composite aerogels, Cellulose, 20(5), pp. 2417–2426, 2013.
  • [14] Saxena, S. & Rai, S., Okara: A Low-Cost Adsorbent for Textile Waste Water Treatment, Res. Biot., 2(2), pp. 26-29, 2020.
  • [15] Elgarahy, A.M., Elwakeel, K.Z., Mohammad, S.H. & Elshoubaky, G.A., A critical review of biosorption of dyes, heavy metals and metalloids from wastewater as an efficient and green process, Clean. Eng. Technol., 4, article number 100209, 2021.
  • [16] Si, R., Pu, J., Luo, H., Wu, C. & Duan, G., Nanocellulose-Based Adsorbents for Heavy Metal Ion, Polymers (Basel)., 14(24), pp. 1–23, 2022.
  • [17] Wang, J. & Chen, C., Chitosan-based biosorbents: Modification and application for biosorption of heavy metals and radionuclides, Bioresour. Technol., 160, pp. 129–141, 2014.
  • [18] Bilal, M., Rasheed, T., Sosa‐Hernández, J.E., Raza, A., Nabeel, F. & Iqbal, H.M.N., Biosorption: An interplay between marine algae and potentially toxic elements—A review, Mar. Drugs, 16(2), pp. 1–16, 2018.
  • [19] Farhan, M., Nurnl, A., Khalid, M., Syazwanie, N. & Aziz, A., Valorization of Okara biosorbent for Heavy Metal Removal, Chemical Engineering, Universiti Teknologi Mara, Selangor, 2015.

  • [20] Hiew, B.Y.Z., Lee, L.Y. & Lee, X.J., Thangalazhy-Gopakumar, S., & Gan, S., Utilisation of environmentally friendly okara-based biosorbent for cadmium(II) removal, Environ. Sci. Pollut. Res., 28(30), pp. 40608– 40622, 2021.
  • [21] Nguyen, T.A.H., Ngo, H.H., Guo, W.S., Nguyen, T.V., Zhang, J., Liang, S., Chen, S.S. & Nguyen, N.C., A comparative study on different metal loaded soybean milk by-product "okara" for biosorption of phosphorus from aqueous solution, Bioresour. Technol., 169, pp. 291–298, 2014.
  • [22] Yu, C., Li, B., Zhang, K., Li, F. & Yan, H., Adsorption capacity of sodium dodecyl sulfate activation okara for methylene blue on aqueous solution, Korean J. Chem. Eng., 39(1), pp. 198–208, 2022.
  • [23] Zhang, P., Yang, M., Lan, J., Huang, Y., Zhang, J., Huang, S., Yang, Y. & Ru, J., Water Quality Degradation Due to Heavy Metal Contamination: Health Impacts and Eco-Friendly Approaches for Heavy Metal Remediation, Toxics, 11(10), pp. 828, 2023.
  • [24] Baldovi, A.A., Ayvazian, A.P., Coelho, L.H.G. & de Jesus, T.A., Biosorption of Pb(II) by Unmodified Banana Peel in Batch and Column Experiments: A Potential Green and Low-Cost Technology for Industrial Effluent Treatment, Water Air Soil. Pollut, 233, pp. 490, 2022.
  • [25] Anwar, J., Shafique, U., Waheed-uz-Zaman, U., Salman, M., Dar, A. & Anwar, S., Removal of Pb(II) and Cd(II) from Water by Adsorption on Peels of Banana, Bioresour. Technol., 101, pp.1752–1755, 2010.
  • [26] Khalil, U., Shakoor, M.B., Ali, S., Ahmad, S.R., Rizwan, M., Alsahli, A. A. & Alyemeni, M., Selective Removal of Hexavalent Chromium from Wastewater by Rice Husk: Kinetic, Isotherm and Spectroscopic Investigation, Water, 13, pp. 263, 2021.
  • [27] Heraldy, E., Lestari, W.W., Permatasari, D. & Arimurti, D., Biosorbent from Tomato Waste and Apple Juice Residue for Lead Removal, J. Environ. Chem. Eng., 6, pp. 1201–1208, 2018.
  • [28] Amar, M.B., Walha, K. & Salvadó, V., Valorisation of Pine Cone as an Efficient Biosorbent for the Removal of Pb(II), Cd(II), Cu(II), and Cr(VI), Adsorpt. Sci. Technol., 2021, Article ID 6678530, 2021.
  • [29] Li, W.C., Law, F.Y. & Chan, Y.H., Biosorption studies on copper (II) and cadmium (II) using pretreated rice straw and rice husk, Environ. Sci. Pollut. Res., 24(10), pp. 8903–8915, 2017.
  • [30] Fertu, D.I., Dragoi, E.N., Bulgariu, L., Curteanu, S. & Gavrilescu, M., Modeling the Biosorption Process of Heavy Metal Ions on Neural Networks, Processes, 10(603), pp. 1–24, 2022.
  • [31] Gao, J., Si, C.,& He, Y., Application of soybean residue (okara) as a lowcost adsorbent for reactive dye removal from aqueous solution, Desalin. Water Treat., 53(18), pp. 2266–2277, 2015.

  • [32] Nguyen, H.T.A. & Pham, T.T., Brilliant Green Biosorption from Aqueous Solutions on Okara: Equilibrium, Kinetic and Thermodynamic Studies, J. Water Environ. Technol., 21(1), pp. 30–40, 2023.
  • [33] Magalhães-Ghiotto, G.A.V., Natal, J.P.S., Nishi, L., Andrade, M.B.de, Gomes, R.G. & Bergamasco, R., Okara and okara modified and functionalized with iron oxide nanoparticles for the removal of Microcystis aeruginosa and cyanotoxin, Environ. Technol., 44(18), pp. 2737–2752, 2023.
  • [34] Gao, J.-F., Wang, J.-H., Yang, C., Wang, S.-Y. & Peng, Y.-Z., Binary biosorption of Acid Red 14 and Reactive Red 15 onto acid treated okara: Simultaneous spectrophotometric determination of two dyes using partial least squares regression, Chem. Eng. J., 171(3), pp. 967–975, 2011.
  • [35] Natal, J.P.S., Cusioli, L.F., Vieira, G.A., Magalhães-Ghiotto, Bergamasco, R., & Gomes, R. G., Removal of methylene blue and safranin orange pollutants from liquid effluents by soy residue, Can. J. Chem. Eng., 101(10), pp. 5561–5575, 2023.
  • [36] Wu, C., McClements, D.J., He, M., Zheng, L., Tian, T., Teng, F. & Li, Y., Preparation and characterization of okara nanocellulose fabricated using sonication or high-pressure homogenization treatments, Carbohydr. Polym., 255, article number 117364, 2021.
  • [37] Phanthong, P., Reubroycharoen, P., Hao, X., Xu, G., Abudula, A & Guan, G., Nanocellulose: Extraction and application, Carbon Resour. Convers., 1(1), pp. 32–43, 2018.
  • [38] Reshmy, R., Thomas, D., Philip, E., Paul, S.A., Madhavan, A., Sindhu, R., Binod, P., Pugazhendhi, A., Sirohi, R., Tarafdar, A. & Pandey, A., Potential of nanocellulose for wastewater treatment, Chemosphere, 281, article number 130738, 2021.
  • [39] Rijal, M.S., Nasir, M., Purwasasmita, B.S. & Asri, L.A.T.W., Cellulose nanocrystals-microfibrils biocomposite with improved membrane performance, Carbohydr. Polym. Technol. Appl., 5, article number 100326, 2023.
  • [40] Li, P., Lei, H., Jian, B., Liu, R., Zhou, M., Wang, Y., Liu, H., Wang, Y. & Zhou, B., Okara Cellulose Nanofibrils Produced by Pretreatment with Sustainable Deep Eutectic Solvent Coupled with Various Mechanical Treatments, Pap. Biomater., 7(2), pp. 46–55, 2022.
  • [41] Tofanica, B.M., Belosinschi, D. & Volf, I., Gels, Aerogels and Hydrogels: A Challenge for the Cellulose-Based Product Industries, Gels, 8(8), pp. 1–17, 2022.
  • [42] Al-Shehri, B.M., Khder, A.E.R.S., Ashour, S.S. & Hamdy, M.S., A review: The utilization of mesoporous materials in wastewater treatment, Mater. Res. Express, 6(12), article number 122002, 2019.

  • [43] Jiang, F. & Hsieh, Y. Lo, Super water absorbing and shape memory nanocellulose aerogels from TEMPO-oxidized cellulose nanofibrils via cyclic freezing-thawing, J. Mater. Chem. A, 2(2), pp. 350–359, 2014.
  • [44] Salama, A., Abouzeid, R., Leong, W.S., Jeevanandam, J., Samyn, P., Dufresne, A., Bechelany, M. & Barhoum, A., Nanocellulose-based materials for water treatment: Adsorption, photocatalytic degradation, disinfection, antifouling, and nanofiltration, Nanomaterials, 11(11), 2021.
  • [45] Ji, Y., Wen, Y., Wang, Z., Zhang, S. & Guo, M., Eco-friendly fabrication of a cost-effective cellulose nanofiber-based aerogel for multifunctional applications in Cu(II) and organic pollutants removal, J. Clean. Prod., 255, article number. 120276, 2020.
  • [46] Mo, L., Shen, Y., Tan, Y. & Zhang, S., Ultralight and shapeable nanocellulose/metal-organic framework aerogel with hierarchical cellular architecture for highly efficient adsorption of Cu(II) ions, Int. J. Biol. Macromol., 193B, pp. 1488–1498, 2021.

Research Intelligence

Data from OpenAlex ↗

Metrics

0.00
FWCIfield-weighted
10th
Percentilevs same year + field
Article
Work type
Open Access

Semantic Profile AI-classified research signals

Institution Network

References

  1. Liu, H.M. & Li, H.Y., Application and Conversion of Soybean Hulls, Soybean - The Basis of Yield, Biomass and Productivity, Minobu Kasai, Intech, pp. 111-132, 2017. DOI: 10.5772/66744
  2. Faisal, M., Gani, A., Mulana, F. & Daimon, H., Treatment and Utilization of Industrial Tofu Waste in Indonesia, Asian J. Chem., 28(3), pp. 501–507, 2016. DOI: 10.14233/ajchem.2016.19372
  3. Mahmud, M.A. & Anannya, F.R., Sugarcane bagasse - A source of cellulosic fiber for diverse applications, Heliyon, 7(8), article number 07771, 2021. DOI: 10.1016/j.heliyon.2021.e07771
  4. Chen, X., Zhang, K., Xiao, L.P., Sun, R.C. & Song, G., Total utilization of lignin and carbohydrates in Eucalyptus grandis: An integrated biorefinery strategy towards phenolics, levulinic acid, and furfural, Biotechnol Biofuels, 13(2), pp. 1–10, 2020. DOI: 10.1186/s13068-019-1644-z
  5. Chen, X., Li, H., Yao, S., Wang, C., Chen, X., Guo, H., Xiong, L., Zhang, H. & Chen, X., The alleviation of lignin inhibition on enzymatic hydrolysis of cellulose by changing its ultrastructure, Industrial Crop. Prod., 185, Article number 115108, 2022. DOI: 10.1016/j.indcrop.2022.115108
  6. Zhu, J., Tan, W.K., Song, X., Gao, Z., Wen, Y., Ong, C.N., Loh, C.S., Swarup, S. & Li, J., Converting Okara to Superabsorbent Hydrogels as Soil Supplements for Enhancing the Growth of Choy Sum (Brassica sp.) under Water-Limited Conditions, ACS Sustain. Chem. Eng., 8(25), pp. 9425–9433, 2020. DOI: 10.1021/acssuschemeng.0c02181
  7. Nishat, A., Yusuf, M., Qadir, A., Ezaier, Y., Vambol, V., Khan, M.I., Moussa, S. Ben, Kamyab, H., Sehgal, S.S., Prakash, C., Yang, H.-H., Ibrahim, H. & Eldin, S.M., Wastewater treatment: A short assessment on available techniques, Alexandria Eng. J., 76, pp. 505–516, 2023.
  8. Bryukhov, M. & Ulrikh, D., Wastewater treatment: Methods and prospects, IOP Conf. Ser. Earth Environ. Sci., 1061(1), article number 012049, 2022. DOI: 10.1088/1755-1315/1061/1/012049
  9. Li, B., Qiao, M. & Lu, F., Composition, Nutrition, and Utilization of Okara (Soybean Residue), Food Rev. Int., 28(3), pp. 231–252, 2012.
  10. Cui, X., Lee, J.J.L. & Chen, W.N., Eco-friendly and biodegradable cellulose hydrogels produced from low cost okara: towards non-toxic flexible electronics, Sci. Rep., 9(1), pp. 1–9, 2019. DOI: 10.1038/s41598-019-54638-5
  11. van der Riet, W.B., Wight, A.W., Cilliers, J.J.L. & Datel, J.M., Food chemical investigation of tofu and its byproduct okara, Food Chem., 34(3), pp. 193–202, 1989.
  12. Mateos-Aparicio, I., Redondo-Cuenca, A., Villanueva-Suárez, M.J., Zapata-Revilla, M.A. & Tenorio-Sanz, M.D., Pea pod, broad bean pod and okara, potential sources of functional compounds, Lwt, 43(9), pp. 1467–1470, 2010. DOI: 10.1016/j.lwt.2010.05.008
  13. Arboleda, J.C., Hughes, M., Lucia, L.A., Laine, J., Ekman, K. & Rojas, O. J., Soy protein-nanocellulose composite aerogels, Cellulose, 20(5), pp. 2417–2426, 2013. DOI: 10.1007/s10570-013-9993-4
  14. Saxena, S. & Rai, S., Okara: A Low-Cost Adsorbent for Textile Waste Water Treatment, Res. Biot., 2(2), pp. 26-29, 2020. DOI: 10.54083/resbio.2.2.2020.26-29
  15. Elgarahy, A.M., Elwakeel, K.Z., Mohammad, S.H. & Elshoubaky, G.A., A critical review of biosorption of dyes, heavy metals and metalloids from wastewater as an efficient and green process, Clean. Eng. Technol., 4, article number 100209, 2021. DOI: 10.1016/j.clet.2021.100209
  16. Si, R., Pu, J., Luo, H., Wu, C. & Duan, G., Nanocellulose-Based Adsorbents for Heavy Metal Ion, Polymers (Basel)., 14(24), pp. 1–23, 2022. DOI: 10.3390/polym14245479
  17. Wang, J. & Chen, C., Chitosan-based biosorbents: Modification and application for biosorption of heavy metals and radionuclides, Bioresour. Technol., 160, pp. 129–141, 2014. DOI: 10.1016/j.biortech.2013.12.110
  18. Bilal, M., Rasheed, T., Sosa‐Hernández, J.E., Raza, A., Nabeel, F. & Iqbal, H.M.N., Biosorption: An interplay between marine algae and potentially toxic elements—A review, Mar. Drugs, 16(2), pp. 1–16, 2018.
  19. Farhan, M., Nurnl, A., Khalid, M., Syazwanie, N. & Aziz, A., Valorization of Okara biosorbent for Heavy Metal Removal, Chemical Engineering, Universiti Teknologi Mara, Selangor, 2015.
  20. Hiew, B.Y.Z., Lee, L.Y. & Lee, X.J., Thangalazhy-Gopakumar, S., & Gan, S., Utilisation of environmentally friendly okara-based biosorbent for cadmium(II) removal, Environ. Sci. Pollut. Res., 28(30), pp. 40608–40622, 2021.
  21. Nguyen, T.A.H., Ngo, H.H., Guo, W.S., Nguyen, T.V., Zhang, J., Liang, S., Chen, S.S. & Nguyen, N.C., A comparative study on different metal loaded soybean milk by-product “okara” for biosorption of phosphorus from aqueous solution, Bioresour. Technol., 169, pp. 291–298, 2014. DOI: 10.1016/j.biortech.2014.06.075
  22. Yu, C., Li, B., Zhang, K., Li, F. & Yan, H., Adsorption capacity of sodium dodecyl sulfate activation okara for methylene blue on aqueous solution, Korean J. Chem. Eng., 39(1), pp. 198–208, 2022. DOI: 10.1007/s11814-021-0880-7
  23. Zhang, P., Yang, M., Lan, J., Huang, Y., Zhang, J., Huang, S., Yang, Y. & Ru, J., Water Quality Degradation Due to Heavy Metal Contamination: Health Impacts and Eco-Friendly Approaches for Heavy Metal Remediation, Toxics, 11(10), pp. 828, 2023. DOI: 10.3390/toxics11100828
  24. Baldovi, A.A., Ayvazian, A.P., Coelho, L.H.G. & de Jesus, T.A., Biosorption of Pb(II) by Unmodified Banana Peel in Batch and Column Experiments: A Potential Green and Low-Cost Technology for Industrial Effluent Treatment, Water Air Soil. Pollut, 233, pp. 490, 2022.
  25. Anwar, J., Shafique, U., Waheed-uz-Zaman, U., Salman, M., Dar, A. & Anwar, S., Removal of Pb(II) and Cd(II) from Water by Adsorption on Peels of Banana, Bioresour. Technol., 101, pp.1752–1755, 2010. DOI: 10.1016/j.biortech.2009.10.021
  26. Khalil, U., Shakoor, M.B., Ali, S., Ahmad, S.R., Rizwan, M., Alsahli, A. A. & Alyemeni, M., Selective Removal of Hexavalent Chromium from Wastewater by Rice Husk: Kinetic, Isotherm and Spectroscopic Investigation, Water, 13, pp. 263, 2021. DOI: 10.3390/w13030263
  27. Heraldy, E., Lestari, W.W., Permatasari, D. & Arimurti, D., Biosorbent from Tomato Waste and Apple Juice Residue for Lead Removal, J. Environ. Chem. Eng., 6, pp. 1201–1208, 2018. DOI: 10.1016/j.jece.2017.12.026
  28. Amar, M.B., Walha, K. & Salvadó, V., Valorisation of Pine Cone as an Efficient Biosorbent for the Removal of Pb(II), Cd(II), Cu(II), and Cr(VI), Adsorpt. Sci. Technol., 2021, Article ID 6678530, 2021. DOI: 10.1155/2021/6678530
  29. Li, W.C., Law, F.Y. & Chan, Y.H., Biosorption studies on copper (II) and cadmium (II) using pretreated rice straw and rice husk, Environ. Sci. Pollut. Res., 24(10), pp. 8903–8915, 2017.
  30. Fertu, D.I., Dragoi, E.N., Bulgariu, L., Curteanu, S. & Gavrilescu, M., Modeling the Biosorption Process of Heavy Metal Ions on Neural Networks, Processes, 10(603), pp. 1–24, 2022.
  31. Gao, J., Si, C.,& He, Y., Application of soybean residue (okara) as a low-cost adsorbent for reactive dye removal from aqueous solution, Desalin. Water Treat., 53(18), pp. 2266–2277, 2015. DOI: 10.1080/19443994.2013.865568
  32. Nguyen, H.T.A. & Pham, T.T., Brilliant Green Biosorption from Aqueous Solutions on Okara: Equilibrium, Kinetic and Thermodynamic Studies, J. Water Environ. Technol., 21(1), pp. 30–40, 2023. DOI: 10.2965/jwet.22-059
  33. Magalhães-Ghiotto, G.A.V., Natal, J.P.S., Nishi, L., Andrade, M.B.de, Gomes, R.G. & Bergamasco, R., Okara and okara modified and functionalized with iron oxide nanoparticles for the removal of Microcystis aeruginosa and cyanotoxin, Environ. Technol., 44(18), pp. 2737–2752, 2023.
  34. Gao, J.-F., Wang, J.-H., Yang, C., Wang, S.-Y. & Peng, Y.-Z., Binary biosorption of Acid Red 14 and Reactive Red 15 onto acid treated okara: Simultaneous spectrophotometric determination of two dyes using partial least squares regression, Chem. Eng. J., 171(3), pp. 967–975, 2011.
  35. Natal, J.P.S., Cusioli, L.F., Vieira, G.A., Magalhães-Ghiotto, Bergamasco, R., & Gomes, R. G., Removal of methylene blue and safranin orange pollutants from liquid effluents by soy residue, Can. J. Chem. Eng., 101(10), pp. 5561–5575, 2023.
  36. Wu, C., McClements, D.J., He, M., Zheng, L., Tian, T., Teng, F. & Li, Y., Preparation and characterization of okara nanocellulose fabricated using sonication or high-pressure homogenization treatments, Carbohydr. Polym., 255, article number 117364, 2021. DOI: 10.1016/j.carbpol.2020.117364
  37. Phanthong, P., Reubroycharoen, P., Hao, X., Xu, G., Abudula, A & Guan, G., Nanocellulose: Extraction and application, Carbon Resour. Convers., 1(1), pp. 32–43, 2018.
  38. Reshmy, R., Thomas, D., Philip, E., Paul, S.A., Madhavan, A., Sindhu, R., Binod, P., Pugazhendhi, A., Sirohi, R., Tarafdar, A. & Pandey, A., Potential of nanocellulose for wastewater treatment, Chemosphere, 281, article number 130738, 2021. DOI: 10.1016/j.chemosphere.2021.130738
  39. Rijal, M.S., Nasir, M., Purwasasmita, B.S. & Asri, L.A.T.W., Cellulose nanocrystals-microfibrils biocomposite with improved membrane performance, Carbohydr. Polym. Technol. Appl., 5, article number 100326, 2023. DOI: 10.1016/j.carpta.2023.100326
  40. Li, P., Lei, H., Jian, B., Liu, R., Zhou, M., Wang, Y., Liu, H., Wang, Y. & Zhou, B., Okara Cellulose Nanofibrils Produced by Pretreatment with Sustainable Deep Eutectic Solvent Coupled with Various Mechanical Treatments, Pap. Biomater., 7(2), pp. 46–55, 2022.
  41. Tofanica, B.M., Belosinschi, D. & Volf, I., Gels, Aerogels and Hydrogels: A Challenge for the Cellulose-Based Product Industries, Gels, 8(8), pp. 1–17, 2022.
  42. Al-Shehri, B.M., Khder, A.E.R.S., Ashour, S.S. & Hamdy, M.S., A review: The utilization of mesoporous materials in wastewater treatment, Mater. Res. Express, 6(12), article number 122002, 2019. DOI: 10.1088/2053-1591/ab52af
  43. Jiang, F. & Hsieh, Y. Lo, Super water absorbing and shape memory nanocellulose aerogels from TEMPO-oxidized cellulose nanofibrils via cyclic freezing-thawing, J. Mater. Chem. A, 2(2), pp. 350–359, 2014. DOI: 10.1039/c3ta13629a
  44. Salama, A., Abouzeid, R., Leong, W.S., Jeevanandam, J., Samyn, P., Dufresne, A., Bechelany, M. & Barhoum, A., Nanocellulose-based materials for water treatment: Adsorption, photocatalytic degradation, disinfection, antifouling, and nanofiltration, Nanomaterials, 11(11), 2021. DOI: 10.3390/nano11113008
  45. Ji, Y., Wen, Y., Wang, Z., Zhang, S. & Guo, M., Eco-friendly fabrication of a cost-effective cellulose nanofiber-based aerogel for multifunctional applications in Cu(II) and organic pollutants removal, J. Clean. Prod., 255, article number. 120276, 2020. DOI: 10.1016/j.jclepro.2020.120276
  46. Mo, L., Shen, Y., Tan, Y. & Zhang, S., Ultralight and shapeable nanocellulose/metal-organic framework aerogel with hierarchical cellular architecture for highly efficient adsorption of Cu(II) ions, Int. J. Biol. Macromol., 193B, pp. 1488–1498, 2021. DOI: 10.1016/j.ijbiomac.2021.10.212