1. Home
  2. Archives
  3. Vol 27 (2020) Issue 2
  4. Articles

Kajian Kapasitas Sambungan Tubular Chord Ganda Digrout Dengan Analisis Elemen Hingga

Abstract

The type of offshore platform for oil and natural gas exploration that is widely used in Indonesia is steel jacket platform. Jacket type platforms are generally made of tubular steel. During the service life, jacket type platforms often suffer damage to the joints. One preferred repair method for platform structure elements is by grouting. In the API RP 2A WSD NORSOK N-004 regulations, the formulations of tubular joint capacity reinforced by grouting are specified. The formulations in the regulations are empirical equations that need to be examined experimentally in the lab or tested by finite element analysis method. In this study, testing using the finite element method is conducted. The discussion is limited to the type of tubular joint with double skin chord. By finite element analysis, the influence of grout thickness, grout strength, inner chord thickness, and outer chord thickness to capacity of tubular joints reinforced with grout is investigated. From the analysis, it was found that the thickness and strength of the grout do not have a significant effect on increasing tubular joint capacity. While the thickness of both the inner and outer chords have a significant effect on increasing the tubular joint capacity. By comparison, the results of finite element method analysis are quite close to the results based on API regulation and in general the API results are more conservative except for cases with out-of-plane bending load.AbstrakTipe anjungan lepas pantai untuk eksplorasi minyak dan gas alam yang banyak dipakai di lepas pantai Indonesia adalah tipe jaket baja. Anjungan tipe jaket umumnya dibuat dari baja tubular. Dalam masa layannya, anjungan tipe jaket sering mengalami kerusakan pada sambungan (joint). Salah satu metode perbaikan yang disukai untuk elemen struktur anjungan adalah dengan di-grout. Dalam peraturan API RP 2A WSD dan NORSOK N-004 telah diberikan formulasi perhitungan kapasitas sambungan tubular yang diperkuat grout. Formulasi pada peraturan-peraturan ini merupakan persamaan-persamaan empiris yang perlu diperiksa dengan eksperimental di lab atau diuji dengan analisis metode elemen hingga. Pada penelitian ini dilakukan pengujian dengan metode elemen hingga. Pembahasan dibatasi pada tipe sambungan tubular dengan batang utama (chord) ganda. Dengan analisis elemen hingga akan dilihat pengaruh tebal grout, kuat grout, tebal chord dalam, dan tebal chord luar terhadap kapasitas sambungan tubular yang diperkuat di-grout. Dari hasil analisis diperoleh bahwa tebal dan kuat grout tidak memberikan pengaruh yang signifikan terhadap peningkatan kapasitas sambungan tubular (tubular joint). Sedangkan tebal chord dalam dan luar keduanya memberikan pengaruh yang signifikan terhadap peningkatan kapasitas sambungan tubular. Dari perbandingan diperoleh hasil-hasil analisis metode elemen hingga cukup mendekati hasil-hasil berdasarkan peraturan API RP 2A WSD dan hasil persamaan API RP 2A WSD umumnya ada pada sisi konservatif kecuali pada kasus beban momen keluar bidang.

Keywords

3.3 Faktor kekuatan fungsi geometri \((Q_u)\)

Faktor kekuatan fungsi geometri \((Q_u)\) suatu sambungan bergantung dari tipe dan dimensi sambungan. Formulasi Qu untuk masing-masing tipe sambungan diberikan pada Tabel 1.

Keterangan:

a. \(Q_{\beta}\) merupakan faktor dimensi yang didefinisikan sebagai berikut :

\[Q_{\beta} = \frac{0.3}{\beta(1 - 0.833\beta)}\] untuk \(\beta > 0.6\)

\(Q_{\beta} = 1,0\) untuk \(\beta \leq 0,6\)

b. \(Q_g\) merupakan faktor jarak (gap) yang didefinisikan berikut:

\[Q_g=1+0.2\left[1-2.8\frac{g}{D}\right]^3\] untuk \(\frac{g}{D}\geq0.5\) tetapi \(Q_g\geq1.0\) \[Q_g=0.13+0.65\phi\gamma^{0.5}\] untuk \(\frac{g}{D}\leq-0.5\)

Dimana, \(\phi = \frac{tF_{y,b}}{TF_{y,c}}\)

Jika \(-0.5 \le \frac{g}{p} \le 0.5\) maka nilai \(Q_g\) harus diinterpolasi

3.4 Faktor kekuatan fungsi beban chord (\(Q_f\))

\(Q_f\) adalah faktor yang memperhitungkan pengaruh beban dan kapasitas chord dalam memikul beban sebagai batang. Untuk penelitian ini dibatasi kasus beban pada chord tidak cukup besar untuk mempengaruhi kekuatan sambungan sehingga diambil \(Q_f=1.0\). Nilai kapasitas sambungan akan dibandingkan dengan hasil analisis metode elemen hingga dengan chord tidak dibebani selain dari batang brace.

3.5 Formulasi untuk sambungan digrout

Dalam peraturan API RP 2A WSD 2007, formulasi kapasitas sambungan digrout diberikan dengan nilai \(Q_u\) yang dimodifikasi. Berdasarkan API RP 2A WSD, untuk sambungan digrout penuh maupun kondisi chord ganda, nilai \(Q_u\) ditunjukkan pada Tabel 2.

Tabel 2 tidak memberikan faktor kapasitas fungsi geometri \((Q_u)\) untuk kapasitas tekan. Hal ini dikarenakan sambungan digrout, terutama tipe grout penuh, sangat kuat menahan gaya tekan sehingga kapasitas sambungan digrout untuk kondisi aksial tekan biasanya lebih besar dari kapasitas batang brace. Dengan kata lain, batang brace lebih dahulu mengalami kegagalan dibandingkan sambungan.

Persamaan pada Tabel 2 dapat dipakai untuk sambungan grout penuh maupun sambungan chord ganda. Tetapi, khusus untuk sambungan chord ganda kegagalan bisa juga terjadi akibat deformasi chord (ovalization). Kapasitas sambungan chord ganda terhadap ovalization dapat diperkirakan dengan persamaan sambungan tanpa grout pada Tabel 1 dengan mengganti ketebalan batang chord (T) dengan ketebalan efektif (\(T_e\)) sesuai Persamaan 3.

\[T_e = \sqrt{T^2 + T_p^2} \tag{3}\]

Keterangan:

T<sub>e</sub>: Ketebalan efektif batang chord ganda

T: Ketebalan batang chord luar (kaki jaket)

\(T_p\): Ketebalan batang chord dalam (tiang pancang)

4. Model Elemen Hingga

Metode elemen hingga (MEH) adalah salah satu metode yang bisa memberikan hasil yang akurat bergantung pada pemodelan objek/permasalahannya. Pada bagian ini dipresentasikan pemilihan elemen dan pembuatan jaring-jaring (mesh) dan kriteria kapasitas yang diterapkan dalam analisis.

Tabel 2. Nilai Qu sambungan digrout berdasarkan API

JenisAksial tarikMomenMomen keluar
Sambungansebidangbidang
Y/K/X\[1,25\beta\gamma(1+\frac{1}{\sin\theta})\]1,5 β γ1,5 β γ

Tabel 1. Faktor kekuatan fungsi geometri (Qu) berdasarkan API RP 2A WSD

Jenis
Sambungan
Aksial tarikAksial tekanMomen sebidangMomen
keluar bidang
K\[(1.6+1.2\gamma)\beta^{1.2}Q_g \leq 40\]\(\boldsymbol{\beta}^{1,2}\boldsymbol{Q}_{g}\)
Y/T30β\(2.8 + (20 + 0.8\gamma)\beta^{1.6}\)_
Y/1зор\(\leq 2.8 + 36\beta^{1.6}\)\[(5+0.7\gamma)\beta^{1.2}\]\(2.5 + (4.5 + 0.2\gamma)\beta^{2.6}\)
Х23\(\beta\) for \(\beta \le 0.9\)
20.7 + \((\beta - 0.9)(17\gamma - 220)\) for \(\beta > 0.9\)
\([2.8 + (12 + 0.1\gamma)\beta]Q_{\beta}\)_

106 Jurnal Teknik Sipil

7LSH HOHPHQ GDQ PRGHO WLSLNDO VDPEXQJDQ WXEXODU

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

*DPEDU-HQLV-MHQLVHOHPHQVROLG$%$486 VXPEHU$%$486

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

6HODLQ SHQJJXQDDQ WLSH HOHPHQ GDODP SHPRGHODQ SHPEDJLDQ HOHPHQ PHVKLQJ MXJD SHUOX VDQJDW PHPSHQJDUXKLDNXUDVLKDVLOPHWRGHHOHPHQKLQJJD3DGD GDVDUQ\D SHPEHQWXNDQMDULQJ-MDULQJ PHVK SDGD GDHUDK GHQJDQ JUDGLHQ WHJDQJDQ \DQJ EHVDU KDUXV OHELK UDSDW .KXVXV VDPEXQJDQ WXEXODU JUDGLHQ WHJDQJDQ WHUEHVDU WHUMDGL SDGD GDHUDK SHUWHPXDQ DQWDUD EDWDQJ EUDFH GHQJDQ EDWDQJ FKRUGVHKLQJJD SHPEDJLDQ HOHPHQ SDGD GDHUDKWHUVHEXWKDUXVOHELKUDSDW

&RQWRK MDULQJ-MDULQJ HOHPHQ KLQJJD XQWXN DQDOLVLV VDPEXQJDQ WXEXODU \DQJ GLSDNDL GDODP SHQHOLWLDQ LQL GLWXQMXNNDQ SDGD *DPEDU 3HUWHPXDQ DQWDUD HOHPHQ EDMD GLJURXW GLPRGHONDQ VHEDJDL HOHPHQ NRQWDN \DQJ KDQ\DHIHNWLIPHQ\DOXUNDQWHJDQJDQWHNDQ$SDELODSDGD GDHUDK SHUWHPXDQ HOHPHQ EDMD GDQ JURXW WHUMDGL NHFHQGHUXQJDQ WHJDQJDQ WDULN PDND DNDQ WLPEXO FHODK JDS DQWDUDNHGXDMHQLVPDWHULDO

*DPEDU-DULQJ-MDULQJHOHPHQKLQJJDVDPEXQJDQWXEXODU

3HQHQWXDQNHJDJDODQVDPEXQJDQWXEXODU

8QWXNPHQHQWXNDQNHJDJDODQVXDWXVDPEXQJDQWXEXODU KDUXV GLWHQWXNDQ VXDWX SDUDPHWHU EDWDV 'DODP SHQHOLWLDQ LQL GLJXQDNDQ VXDWX EDWDV GHIRUPDVL XQWXN PHQHQWXNDQ NDSDVLWDV VDPEXQJDQ WXEXODU %DWDV GHIRUPDVL \DQJ GLJXQDNDQ \DLWX <XUD 'HIRUPDWLRQ /LPLW6ZHQVVRQGDQ<XUD3HFNQROGHWDO %DWDV GHIRUPDVL <XUD LQL PHPEHULNDQ EDWDVDQ SHUSLQGDKDQ GDQ URWDVL \DQJ WHUMDGL SDGD MRLQ WXQJJDO VHSHUWLMRLQ7 GDQMRLQ<%DWDV GHIRUPDVL<XUD <XUD GHIRUPDWLRQOLPLW GLWXQMXNNDQSDGD3HUVDPDDQGDQ

%DWDVSHUSLQGDKDQ<XUD\DLWX

Batas rotasi Yura, yaitu \[\phi_{Yura} = \frac{80F_y}{E_z}\]

6WXGL.DVXV

'HVNULSVLPRGHO

'DODP SHQHOLWLDQ LQL DNDQ GLWLQMDX VDPEXQJDQ WXEXODU XQWXN EHUEDJDL YDULDVL \DQJ GLPRGHONDQ GHQJDQ NRQILJXUDVLVHSHUWLGLWXQMXNNDQ*DPEDU

8QWXN PHOLKDW KXEXQJDQ DQWDUD NHWHEDODQ JURXW GDQ NHNXDWDQ JURXW WHUKDGDS NDSDVLWDV VDPEXQJDQ WXEXODU PDND GLEXDW EHEHUDSD PRGHO VDPEXQJDQ WXEXODU GHQJDQ YDULDVL NHWHEDODQ JURXW GDQ YDULDVL NHNXDWDQ

23

*DPEDU.RQILJXUDVLGDQGLPHQVLVDPEXQJDQWXEXODU

grout. Selain itu, pada penelitian ini juga dimodelkan beberapa sambungan tubular dengan variasi ketebalan batang chord luar dan variasi ketebalan batang chord dalam. Masing-masing dibuat 3 variasi model untuk melihat perbandingan peningkatan kapasitasnya sehingga total model sambungan tubular yaitu 12 model. Rangkuman model sambungan tubular yang dimodelkan ditunjukkan pada Tabel 3. Pada Tabel 3, angka merah menunjukkan variabel yang divariasikan untuk setiap kelompok. Untuk semua model dilakukan analisis digrout dan tanpa grout. Apabila suatu model dianalisis untuk kondisi tanpa grout, model grout dan chord dalam tidak diaktifkan.

5.2 Model material

Dalam studi kasus ini digunakan dua jenis material yaitu material baja dan material grout. Untuk semua model, material baja yang dipakai pada kondisi elastisnya mempunyai modulus elastisitas E=200000 MPa, Poisson rasio v=0,3 dan tegangan leleh \(F_y=320\) MPa. Pada kondisi plastis dipakai model dengan strain hardening dan regangan putus 20%. Hubungan tegangan dan regangan baja pada kondisi plastis ditunjukkan pada Gambar 5.

Untuk material grout dimodelkan tiga variasi kekuatan yaitu f<sub>c</sub>'=41,5 MPa, f<sub>c</sub>'=62,25 MPa, dan f<sub>c</sub>'=83 MPa. Untuk membuat kurva tegangan regangan grout digunakan model yang diusulkan oleh Thorenfeldt et. al. (1987). Menurut model ini hubungan tegangan (f<sub>c</sub>)

Tabel 3. Deskripsi model sambungan tubular

ModelChordluar BraceChord dalamTebal
grout
Kuat
grout
D [mm]T
[mm]
d
[mm]
t [mm]Dp [mm]Tp [mm]tg
[mm]
fc'
[MPa]
190025350108252512,541,5
Α29002535010800252541,5
39002535010750255041,5
19002535010800252541,5
В29002535010800252562,25
39002535010800252583
1900253501080012,52541,5
С29002535010800252541,5
39002535010800502541,5
187512,535010800252541,5
D29002535010800252541,5
39505035010800252541,5
7

Gambar 5. Kurva tegangan regangan plastis baja

dan regangan (e) ditunjukkan pada Persamaan 5. Hasil plot model ini untuk tiga macam kekuatan grout ditunjukkan pada Gambar 6.

\[\frac{f_c}{f_c'} = \frac{\varepsilon_c}{\varepsilon_c'} \frac{n}{n - 1 + \left(\frac{\varepsilon_c}{\varepsilon_c'}\right)^{nk}}\] (5)

dimana,

\[k = 1 \quad \text{untuk}^{\varepsilon_c}/_{\varepsilon_c'} \le 1\] \[k = 0.67 + \frac{f_c'}{62} \quad \text{untuk}^{\varepsilon_c}/_{\varepsilon_c'} > 1\] \[n = 0.4 \times 10^{-3} f_c' \text{ (psi)} + 1.0\]

13

Gambar 6. Kurva tegangan regangan grout

Model klasik plastisitas von Mises dipergunakan untuk baja. Model menerapkan permukaan leleh von Mises yang diasosiasikan dengan aliran plastik untuk leleh isotropis dan hardening. Formulasi detail model ini dapat dilihat antara lain pada manual ABAQUS (ABAQUS 2011) dan Wei (2011).

Model untuk grout ditentukan dengan menerapkan kurva uni-aksial pada Gambar 6 ke model material concrete damaged plasticity pada perangkat lunak ABAQUS. Model concrete damaged plasticity memberikan kemampuan umum untuk pemodelan beton dan material quasi-getas lain pada struktur. Detail dan dasar teori model material ini dapat dilihat antara lain pada manual ABAQUS (ABAQUS 2011) dan Wei (2011).

5.3 Verifikasi tipe elemen hingga

Untuk memastikan model elemen hingga yang dipakai sudah memberikan akurasi yang memadai, dilakukan verifikasi jumlah lapisan elemen dan tipe elemen. Verifikasi yang dilakukan adalah untuk mempelajari jenis elemen dan meshing yang efisien untuk mendapatkan konvergensi hasil dengan usaha komputasi minimal. Dua jenis elemen yang disediakan ABAQUS dibandingkan, yaitu elemen C3D8I dan C3D20R. Jumlah lapis elemen untuk diskritisasi baja dan grout juga dibandingkan dengan memvariasikan jumlah lapisan elemen dari 1 lapis, 2 lapis sampai dengan 4 lapis. Verifikasi banyaknya lapisan elemen

SDGD PHVKLQJ NHWHEDODQ EDMD GDQ JURXW GLODNXNDQ PHQJLQJDW WHUMDGLQ\D JD\D GDODP PRPHQ VHPHQWDUD \DQJ GLSDNDL DGDODK HOHPHQ ' EULFN EXNDQ FDQJNDQJ VKHOO 9HULILNDVLGHQJDQPHPEDQGLQJNDQWHUKDGDSKDVLO H[SHULPHQWDO WLGDN GLODNXNDQ NDUHQD NHWHUEDWDVDQ OLQJNXS VWXGL GDQ MXJD NHWHUEDWDVDQ GDWD \DQJ WHUVHGLD +DVLO SHUEDQGLQJDQ SDGD YHULILNDVL LQL XQWXN NDSDVLWDV WHNDQGDQPRPHQVHELGDQJGLWXQMXNNDQSDGD*DPEDU GDQ

'DUL NXUYD-NXUYD SDGD *DPEDU GDQ GDSDW GLOLKDW EDKZD NDSDVLWDV GDQ NXUYD NDSDVLWDV GHQJDQ GXD WLSH

3

*DPEDU3HUEDQGLQJDQNXUYDJD\DWHNDQIXQJVL SHUSLQGDKDQXQWXNEHEHUDSDWLSHMDULQJ-MDULQJHOHPHQKLQJJD

5

*DPEDU3HUEDQGLQJDQNXUYDPRPHQIXQJVLURWDVLXQWXN EHEHUDSDWLSHMDULQJ-MDULQJHOHPHQKLQJJD

HOHPHQ GDQ MXPODK ODSLVDQ \DQJ EHUEHGD PHPEHULNDQ KDVLO\DQJWLGDNMDXKEHUEHGD'HQJDQPHPEDQGLQJNDQ NDSDVLWDV XQWXN PRGHO GHQJDQ OD\HU GDQ WLSH HOHPHQ PHVKLQJ \DQJEHUEHGDGLSHUROHKUDWD-UDWDSHUVHQVHOLVLK VHNLWDU 'HQJDQ GHPLNLDQ GDSDW GLVLPSXONDQ SHQJJXQDDQHOHPHQPHVKLQJ WLSH&',GHQJDQVDWX ODSLVDQ DGDODK \DQJ WHUEDLN NDUHQD VXGDK PHPEHULNDQ KDVLO \DQJ FXNXS DNXUDW GHQJDQ UXQQLQJ WLPH \DQJ PLQLPDO

'LVWULEXVL WHJDQJDQ GDQ NXUYD NDSDVLWDV KDVLO DQDOLVLVPHWRGHH(OHPHQKLQJJD

%HULNXW LQL GLWXQMXNNDQ GLVWULEXVL WHJDQJDQ GDQ NXUYD JD\DPRPHQ VHEDJDL IXQJVL SHUSLQGDKDQURWDVL XQWXN VDWXFRQWRK NDVXVSDGD VHWLDSWLSHSHPEHEDQDQ8QWXN PRGHOQ\D GLSLOLK PRGHO ' GDQ GLEDQGLQJNDQ DQWDUD NRQGLVL WDQSD JURXW GDQ GLJURXW 'LVWULEXVL WHJDQJDQ GLWXQMXNNDQGHQJDQZDUQD-ZDUQDEHUEHGD%DJLDQ\DQJ EHUZDUQD PHUDK PHQJDODPL WHJDQJDQ PDNVLPXP :DUQD NXQLQJ KLMDX GDQ ELUX VHFDUD EHUXUXWDQ PHQXQMXNNDQWHJDQJDQ\DQJ VHPDNLQNHFLO3DGDEDWDV NHNXDWDQ EDJLDQ \DQJ EHUZDUQD PHUDK VXGDK PHQFDSDLWHJDQJDQOHOHK

3DGD VHWLDS PRGHO SHPEHEDQDQ VWUXNWXU PHQJDODPL WHJDQJDQ VDPSDL SDGD EDWDV OHOHK WDULN PDXSXQ WHNDQ 7HJDQJDQOHOHKLQLWHUVHEDUSDGDGDHUDK-GDHUDKGHQJDQ WHJDQJDQ PDNVLPXP WHWDSL UHJDQJDQ EHOXP PHQFDSDL UHJDQJDQ SXWXV %DWDV NHNXDWDQ GLQ\DWDNDQ WHUFDSDL DSDELOD GHIRUPDVL SHUSLQGDKDQ DWDX URWDVL WHODK PHQFDSDLEDWDVDQ\DQJGLWHQWXNDQGHQJDQEDWDVDQ<XUD 3HUVDPDDQ GDQ

/HOHK \DQJ WHUMDGL SDGD WLWLN-WLWLN GHQJDQ NRQVHQWUDVL WHJDQJDQ WLQJJL PHQ\HEDENDQ NXUYD EHEDQ YV GHIRUPDVL PHOHQJNXQJ GDQ PHQMDGL VHPDNLQ ODQGDL EHUVDPDDQ GHQJDQ PDNLQ EDQ\DNQ\D HOHPHQ \DQJ PHQJDODPL OHOHK .RQVHQWUDVL WHJDQJDQ WLGDN

12

*DPEDU'LVWULEXVLWHJDQJDQGDQGHIRUPDVLDNLEDWJD\DDNVLDOWDULNXQWXN0RGHO'WDQSDJURXWGDQ0RGHO'GLJURXW

1

*DPEDU.DSDVLWDVWDULNXQWXN0RGHO'WDQSDJURXW GDQ0RGHO'GLJURXW

3

*DPEDU.DSDVLWDVWHNDQXQWXNPRGHO'WDQSDJURXW GDQPRGHO'GLJURXW

5

*DPEDU'LVWULEXVLWHJDQJDQGDQGHIRUPDVLDNLEDWJD\DDNVLDOWHNDQXQWXNPRGHO'WDQSDJURXWGDQPRGHO'GLJURXW

7

*DPEDU'LVWULEXVLWHJDQJDQGDQGHIRUPDVLDNLEDWPRPHQVHELGDQJXQWXN0RGHO'WDQSDJURXWGDQ0RGHO'GLJURXW

Jurnal Teknik Sipil

1

*DPEDU.DSDVLWDVPRPHQVHELGDQJXQWXN0RGHO' WDQSDJURXWGDQ0RGHO'GLJURXW

3

*DPEDU.DSDVLWDVPRPHQNHOXDUELGDQJXQWXN0RGHO 'WDQSDJURXWGDQ0RGHO'GLJURXW

5

*DPEDU'LVWULEXVLWHJDQJDQGDQGHIRUPDVLDNLEDWPRPHQNHOXDUELGDQJXQWXN0RGHO'WDQSDJURXWGDQ0RGHO'GLJURXW

PHQLPEXONDQ NHJDJDODQ SUHPDWXU NDUHQD VLIDW GDNWDLO PDWHULDOEDMD

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

%HEDQDNVLDOWDULN

'LVWULEXVLWHJDQJDQDNLEDWEHEDQDNVLDOWDULNSDGDEDWDQJ EUDFH GLWXQMXNNDQ SDGD *DPEDU +DVLO XQWXN PRGHO WDQSD JURXW GDQ GLJURXW GLWXQMXNNDQ EHUVHEHODKDQ SDGD *DPEDU .XUYD JD\D DNVLDO VHEDJDL IXQJVL SHUSLQGDKDQGLWXQMXNNDQSDGD*DPEDU.XUYDXQWXN NRQGLVL GHQJDQ GDQWDQSD JURXW GLEDQGLQJNDQ SDGD VDWX JDPEDU *DULV YHUWLNDO PHQXQMXNNDQ EDWDV GHIRUPDVL <XUD \DQJ GLSDNDL VHEDJDL EDWDV NHJDJDODQ VDPEXQJDQ

6ZHQVVRQ GDQ <XUD 'HIRUPDVL \DQJ WHUMDGL PHQXQMXNNDQ WLPEXOQ\D FHODK JDS DQWDUD FKRUG OXDU GLJURXW VHKLQJJD NDSDVLWDV VDPEXQJDQ GLWHQWXNDQ ROHK NHNXDWDQ SXQFKLQJ VKHDU FKRUG OXDU )XQJVL JURXW GDODP KDO LQL DGDODK PHQLQJNDWNDQ NHWDKDQDQ VDPEXQJDQ PHQDKDQ GHIRUPDVL RYDO RYDOL]DWLRQ VHKLQJJD NDSDVLWDV VDPEXQJDQ DNDQ PHQLQJNDW DNLEDW JURXW DSDELOD RYDOL]DWLRQ PHUXSDNDQ NHJDJDODQ NULWLV GDQEXNDQSXQFKLQJVKHDU

%HEDQDNVLDOWHNDQ

'LVWULEXVL WHJDQJDQ DNLEDW EHEDQ DNVLDO WHNDQ SDGD EDWDQJ EUDFH GLWXQMXNNDQ SDGD *DPEDU +DVLO XQWXN PRGHO WDQSD JURXW GDQ GLJURXW GLWXQMXNNDQ EHUVHEHODKDQ SDGD *DPEDU .XUYD JD\D DNVLDO VHEDJDL IXQJVL SHUSLQGDKDQ GLWXQMXNNDQ SDGD*DPEDU .XUYD XQWXN NRQGLVL GHQJDQ GDQ WDQSD JURXW GLEDQGLQJNDQ SDGD VDWX JDPEDU *DULV YHUWLNDO PHQXQMXNNDQ EDWDV GHIRUPDVL <XUD \DQJ GLSDNDL VHEDJDL EDWDV NHJDJDODQ VDPEXQJDQ 6ZHQVVRQ GDQ <XUD $NLEDW EHEDQ DNVLDOWHNDQWHJDQJDQ \DQJ WHUMDGL SDGD GDHUDK VDPEXQJDQ DGDODK WHJDQJDQ WHNDQ VHKLQJJD WLGDN DGD PDVDODK WHUEHQWXNQ\D FHODK JDS DQWDUD EDMD GLJURXW 'HQJDQ NRQGLVL LQL FKRUG OXDU

JURXW GDQ FKRUG GDODP EHNHUMD VDPD PHQDKDQ EHEDQ VHKLQJJD NDSDVLWDV VDPEXQJDQ QDLN GUDVWLV 3HQLQJNDWDQ NDSDVLWDV VDPEXQJDQ GLEDWDVL MXJD ROHK NHPXQJNLQDQRYDOL]DWLRQEHUEHGDGLJURXWSHQXK\DQJ PHQJXEDKFKRUG PHQMDGLOLQJNDUDQVROLG

%HEDQPRPHQVHELGDQJ

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

%HEDQPRPHQNHOXDUELGDQJ

'LVWULEXVLWHJDQJDQDNLEDWEHEDQPRPHQNHOXDUELGDQJ SDGDEDWDQJEUDFHGLWXQMXNNDQSDGD*DPEDU +DVLO XQWXN PRGHO WDQSD JURXW GDQ GLJURXW GLWXQMXNNDQ EHUVHEHODKDQ SDGD *DPEDU .XUYD PRPHQ NHOXDU

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

3HUEDQGLQJDQ KDVLO PHWRGH HOHPHQ KLQJJD GHQJDQIRUPXODVL$3,

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

3DGD 7DEHO GLSUHVHQWDVLNDQ KDVLO-KDVLO DQDOLVLV GHQJDQ PHWRGH HOHPHQ KLQJJD 0(+ GDQ GHQJDQ

0RGHO$NVLDO7DULN >N1@$NVLDO7HNDQ >N1@0RPHQ6HELGDQJ >N1P@0RPHQ.HOXDU%LGDQJ >N1P@
0(+$3,0(+$3,0(+$3,0(+$3,
'
'
'
6HOLVLKUDWD-UDWD

7DEHO.DSDVLWDVVDPEXQJDQWXEXODUGLJURXWKDVLODQDOLVLVHOHPHQKLQJJDGDQIRUPXODVL$3,53$:6'

0RGHO$NVLDO7DULN >N1@$NVLDO7HNDQ >N1@0RPHQ6HELGDQJ >N1P@0RPHQ.HOXDU%LGDQJN1P@
0(+$3,0(+$3,0(+$3,0(+$3,
$
$
$
%
%
%
&
&
&
'
'
'
6HOLVLKUDWD-UDWD

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Ȗ VHGLNLW GLOXDU EDWDV YDOLGLWDV IRUPXODVL \DLWX +DO LQL PHQMDGL SHULQJDWDQ EDKZD EDWDV YDOLGLWDV \DQJ GLWHQWXNDQ SDGD VXDWXIRUPXODVLKDUXVVHODOXGLSHQXKL

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

$QDOLVLVSHQLQJNDWDQNDSDVLWDVDNLEDWJURXW

%HUGDVDUNDQ KDVLO DQDOLVLV PHWRGH HOHPHQ KLQJJD GLODNXNDQ SHUKLWXQJDQ SHQLQJNDWDQ NDSDVLWDV DNLEDW DGDQ\D JURXW XQWXN PDVLQJ-PDVLQJ PRGHO 5DQJNXPDQ SHQLQJNDWDQ NDSDVLWDV VDPEXQJDQ WXEXODU FKRUG JDQGD VHWHODK GLJURXW GLEDQGLQJNDQ GHQJDQ NDSDVLWDV VHEHOXP GLJURXW GLWXQMXNNDQ SDGD 7DEHO +DVLO LQL PHQXQMXNNDQ SHQLQJNDWDQ NDSDVLWDV \DQJ FXNXS EHVDU GDULDSOLNDVLJURXWSDGDVDPEXQJDQWXEXODUFKRUG JDQGD 3HUVHQWDVH SHQLQJNDWDQ NDSDVLWDV WHUEHVDU GLWXQMXNNDQ SDGDNDVXVEHEDQDNVLDOWHNDQ

$QDOLVLV SDUDPHWHU NDSDVLWDV VDPEXQJDQ WXEXODU FKRUG JDQGDGLJURXW

8QWXN ELVD PHQXQMXNNDQ SHQJDUXK SDUDPHWHU-SDUDPHWHU VDPEXQJDQ WXEXODU \DQJ EHUSHUDQ GDODP NDSDVLWDV VDPEXQJDQ WXEXODU FKRUG JDQGD GLJURXW KDVLO-KDVLO DQDOLVLV GLSUHVHQWDVLNDQ GDODP NXUYD-NXUYD EHUGDVDUNDQ SDUDPHWHU \DQJ LQJLQ GLWLQMDX GL EDZDK LQL 8QWXN SUHVHQWDVLNDSDVLWDVJD\DDNVLDOGDQPRPHQGLSORWSDGD

7DEHO3HQLQJNDWDQNDSDVLWDVVDPEXQJDQWXEXODUFKRUG JDQGDDNLEDWJURXW

3HQLQJNDWDQ.DSDVLWDV
0RGHO7DULN7HNDQ0RPHQ
6HELGDQJ
0RPHQ.HOXDU
%LGDQJ
>@>@>@>@
$
$
$
%
%
%
&
&
&
'
'
'

JUDILN \DQJ VDPD GDQ VNDOD PRPHQ GLEXDW [ DJDU JUDILNQ\DOHELKVHWDUD

3DUDPHWHUWHEDOJURXW

0RGHO VHW $ PHUXSDNDQ PRGHO GHQJDQ NHWHEDODQ JURXW \DQJ EHUEHGD GDQ SDUDPHWHU ODLQQ\D NRQVWDQ 'LSLOLK NHWHEDODQ JURXWPHUXSDNDQ NHOLSDWDQGDULWHEDO FKRUG OXDU \DLWX0RGHO $ VDPSDL0RGHO $ GHQJDQ WHEDO JURXW PDVLQJ-PDVLQJ 7 7 GDQ 7 .XUYD KXEXQJDQ DQWDUD NDSDVLWDV VDPEXQJDQ WXEXODU GLJURXW VHEDJDL IXQJVL WHEDO JURXW GLWXQMXNNDQ SDGD *DPEDU

'DUL *DPEDU GDSDW GLOLKDW EDKZD GHQJDQ EHUWDPEDKQ\D NHWHEDODQ JURXW EHUWDPEDK SXOD NDSDVLWDV VDPEXQJDQ +DO WHUVHEXW PHQXQMXNNDQ NHWHEDODQ JURXW PHPEHULNDQ SHQJDUXK WHUKDGDS NDSDVLWDVSDGDVDPEXQJDQWXEXODUFKRUG JDQGDGLJURXW 1DPXQ SHUXEDKDQ NHWHEDODQ JURXW WLGDN PHPEHULNDQ SHQJDUXK \DQJ EHJLWX VLJQLILNDQ SDGD SHQLQJNDWDQ NDSDVLWDV VDPEXQJDQ WXEXODU +DO LQL VHVXDL GHQJDQ IRUPXODVL GDODP SHUDWXUDQ $3, 53 $ :6' GDQ 12562. 1- \DQJ WLGDN PHPSHUKLWXQJNDQ SHQJDUXKNHWHEDODQJURXW

13

*DPEDU.DSDVLWDVVDPEXQJDQWXEXODUGLJURXWIXQJVL WHEDOJURXW

3DUDPHWHUNXDWPDWHULDOJURXW

0RGHO VHW % PHUXSDNDQ PRGHO GHQJDQ NHNXDWDQ PDWHULDO JURXW \DQJ EHUEHGD GDQ SDUDPHWHU ODLQQ\D NRQVWDQ.XUYDKXEXQJDQDQWDUDNDSDVLWDVVDPEXQJDQ WXEXODU GLJURXW VHEDJDL IXQJVL NXDW PDWHULDO JURXW GLWXQMXNNDQSDGD*DPEDU

3

*DPEDU.DSDVLWDVVDPEXQJDQWXEXODUGLJURXWIXQJVL NXDWPDWHULDOJURXW

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

3DUDPHWHUWHEDOFKRUGGDODP

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

'DUL *DPEDU GDSDW GLOLKDW EDKZD GHQJDQ EHUWDPEDKQ\D NHWHEDODQ HIHNWLI DNLEDW EHUWDPEDKQ\D NHWHEDODQ FKRUG GDODP EHUWDPEDK SXOD NDSDVLWDV VDPEXQJDQ WXEXODU GLJURXW 3HQLQJNDWDQ NDSDVLWDV JD\D WHNDQ PHQXQMXNNDQ JUDGLHQ NRQVWDQ \DQJ PHQXQMXNNDQ NHNXDWDQ WHNDQ VDQJDW EDLN PHPDQIDDWNDQ JDEXQJDQ FKRUG OXDU GDQ GDODP 6HPHQWDUD SHQLQJNDWDQ NDSDVLWDV XQWXN JD\D DNVLDO WDULN GDQ PRPHQ WHUOLKDW QDLN ODOX PHODQGDL GDQ FHQGHUXQJ NRQVWDQ SDGD NHWHEDODQ HIHNWLI \DQJ PHQLQJNDW +DO LQL PHQXQMXNNDQ DGD NHWHUEDWDVDQ SHQLQJNDWDQNDSDVLWDVNDUHQDFKRUG OXDUJDJDOEHNHUMD

9

*DPEDU.DSDVLWDVVDPEXQJDQIXQJVLNHWHEDODQHIHNWLI GHQJDQNHWHEDODQFKRUGOXDUNRQVWDQ

VHEDJDL VDWX NHVDWXDQ GHQJDQ FKRUG GDODP 3DGD NHWHEDODQ HIHNWLI \DQJ WLQJJL SHQLQJNDWDQ NHNXDWDQ GLEDWDVL ROHK NDSDVLWDV FKRUG OXDU +DO LQL VHVXDL GHQJDQ IRUPXODVL GDODP SHUDWXUDQ $3, 53 $ :6' GDQ 12562. 1- \DQJ PHPSHUKLWXQJNDQ SHQJDUXK NHWHEDODQ FKRUG OXDU GDQ NHWHEDODQ HIHNWLI GDODP GXD VHW SHUVDPDDQ EHUEHGD +DUXV GLFHN NHGXDQ\D GDQ KDUXV GLSDNDL QLODL NDSDVLWDV PLQLPXP DQWDUDKDVLONHGXDQ\D

3DUDPHWHUWHEDOFKRUG OXDU

0RGHO VHW ' PHUXSDNDQ PRGHO GHQJDQ NHWHEDODQ FKRUG OXDU \DQJ EHUEHGD GDQ SDUDPHWHU ODLQQ\D NRQVWDQ 0HQJLNXWL SHPEDKDVDQ VHEHOXPQ\D SHQJDUXK NHWHEDODQ FKRUG OXDU MXJD GLEDKDV GHQJDQ IRUPXODVL NHWHEDODQ HIHNWLI .XUYD KXEXQJDQ DQWDUD NDSDVLWDV VDPEXQJDQ WXEXODU GLJURXW VHEDJDL IXQJVL NHWHEDODQ HIHNWLI GHQJDQ NHWHEDODQ FKRUG GDODP NRQVWDQGLWXQMXNNDQSDGD*DPEDU

14

*DPEDU.DSDVLWDVVDPEXQJDQIXQJVLNHWHEDODQHIHNWLI GHQJDQNHWHEDODQFKRUGGDODPNRQVWDQ

'DUL *DPEDU GDSDW GLOLKDW EDKZD GHQJDQ EHUWDPEDKQ\D NHWHEDODQ HIHNWLI GDQ NHWHEDODQ FKRUG GDODP WHWDS SHQLQJNDWDQ NDSDVLWDV QDLN PRQRWRQ %HUEHGD GHQJDQ KDVLO PHQDLNNDQ NHWHEDODQ FKRUG GDODP VDMD SDGD NDVXVX LQL NHQDLNDQ NDSDVLWDV VDPEXQJDQWLGDN PHODQGDL GDQ PHQMDGL NRQVWDQ SDGD NHWHEDODQ HIHNWLI \DQJ EHVDU +DO LQL EHUEHGD NDUHQD SDGD NDVXV LQL SHQDPEDKDQ NHWHEDODQ HIHNWLI GLEXDW GHQJDQ SHQDPEDKDQ NHWHEDODQ FKRUG OXDU VHKLQJJD NHJDJDODQFKRUG OXDUWLGDNPHQMDGLSHPEDWDVNHQDLNDQ

NDSDVLWDV *UDGLHQ NHQDLNDQ NDSDVLWDVWHUOLKDW PHQXUXQ PHQXQMXNNDQ PDQIDDW NRPSRVLW DQWDUD FKRUG OXDU GDQ FKRUG GDODPPHQXUXQXQWXNNDVXVFKRUGOXDUMDXKOHELK WHEDO GDUL FKRUG GDODP 7HWDSL GDUL JUDILN WHUOLKDW NDSDVLWDV KDPSLU PHUXSDNDQ IXQJVL OLQLHU WHUKDGDS NHWHEDODQHIHNWLI+DOLQLFXNXSVHVXDLGHQJDQ IRUPXODVL GDODPSHUDWXUDQ$3,53$:6'GDQ12562.1- \DQJ PHPSHUKLWXQJNDQ SHQJDUXK NHWHEDODQ FKRUG OXDU WHUKDGDSNDSDVLWDVVHEDJDLIXQJVLOLQLHU

.HVLPSXODQ

'DODPSHQHOLWLDQLQLGLODNXNDQNDMLDQWHUKDGDSNDSDVLWDV VDPEXQJDQ WXEXODU WDQSD GDQ GLJURXW GHQJDQ PHWRGH HOHPHQ KLQJJD GDQ KDVLOQ\D MXJD GLSDNDL XQWXN PHQJHYDOXDVL IRUPXODVL NDSDVLWDV VDPEXQJDQ WXEXODU PHQXUXW SHUDWXUDQ $3, 53 $ :6' 8QWXN SHQHOLWLDQ LQL VLVWHP VDPEXQJDQWXEXODUGDQPHWRGHJURXWGLEDWDVL SDGD VLVWHP GHQJDQ FKRUG JDQGD GRXEOH VNLQ WXEXODU MRLQW %HUGDVDUNDQKDVLODQDOLVLVGDSDWGLDPELOEHEHUDSD NHVLPSXODQVHEDJDLEHULNXW

  • 8QWXN NDVXV VDPEXQJDQ WDQSD JURXW KDVLO-KDVLO PHWRGH HOHPHQ KLQJJD GDQ KDVLO-KDVLO GHQJDQ IRUPXODVL $3, 53 $ :6' PHPEHULNDQ SHUEHGDDQ UDWD-UDWD OHELK NHFLO GDUL 8PXPQ\D KDVLO IRUPXODVL $3, DGD SDGD VLVL NRQVHUYDWLI NHFXDOL SDGD VDWX NDVXV \DQJWLGDN PHPHQXKL EDWDV YDOLGLWDV SHUVDPDDQ $3, +DVLOLQL PDVLK ELVD GLWHULPD NDUHQD KDVLO IRUPXODVL $3, DGD SDGD VLVL NRQVHUYDWLI GDQ UXPXVHPSLULVSHUOXGLEXDWGHQJDQEHQWXNWLGDNWHUODOX NRPSOHNV
  •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
  • 6HPXD PRGHO VDPEXQJDQ FKRUG JDQGD GLJURXW GDQ VHPXD WLSH SHPEHEDQDQ PHQXQMXNNDQ JURXW GDSDW PHQLQJNDWNDQNDSDVLWDVVDPEXQJDQWXEXODU.HQDLNDQ NDSDVLWDVPLQLPXP \DQJ GLDPDWL DGDODK VHNLWDU VHPHQWDUD \DQJ WHUEHVDU ELVD OHELK GDUL 3HUVHQWDVHSHQLQJNDWDQNDSDVLWDVWHUEHVDUGLWXQMXNNDQ SDGDNDVXVEHEDQDNVLDOWHNDQ
  • 3HUXEDKDQNHWHEDODQJURXWGDQNXDWJURXWPHPEHULNDQ SHQJDUXK \DQJ WLGDN EHJLWX VLJQLILNDQ WHUKDGDS SHQLQJNDWDQNDSDVLWDVVDPEXQJDQWXEXODUFKRUGJDQGD

  • GLJURXW +DVLO LQL VHVXDL GHQJDQ SHUDWXUDQ $3, GDQ 12562. \DQJ WLGDN PHQXQMXNNDQ SHQJDUXK WHEDO JURXW GDQ NXDW PDWHULDO JURXW GDODP IRUPXODVL NDSDVLWDVVDPEXQJDQWXEXODU\DQJGLJURXW
  • 3HQDPEDKDQ NHWHEDODQ HIHNWLI GHQJDQ SHQDPEDKDQ NHWHEDODQ FKRUG GDODP VDMD PHPEHULNDQ SHQDPEDKDQ NDSDVLWDV \DQJ FXNXS VLJQLILNDQ WHUKDGDS NDSDVLWDV VDPEXQJDQ WXEXODU GLJURXW .HQDLNDQ NDSDVLWDV PHODQGDL GDQ PHQMDGL NRQVWDQ SDGD VDDW NHJDJDODQ VDPEXQJDQ GLWHQWXNDQ ROHK NHJDJDODQ FKRUG OXDU VHKLQJJD SHQDPEDKDQ NHWHEDODQ FKRUG GDODP WLGDN ELVD PHQLQJNDWNDQ NDSDVLWDV ODJL +DO LQL VHVXDL GHQJDQ SHUXPXVDQ SHUDWXUDQ $3, 53 $ :6' GDQ 12562. 1- \DQJ PHQJKDUXVNDQ SHQJHFHNDQ NDSDVLWDV EHUGDVDUNDQ GXD SHUVDPDDQ EHUEHGD \DQJ SHUWDPD EHUGDVDUNDQ NHWHEDODQ FKRUG OXDU GDQ \DQJ NHGXD EHUGDVDUNDQNHWHEDODQFKRUGHIHNWLIJDEXQJDQ
  • 3HQDPEDKDQ NHWHEDODQ HIHNWLI GHQJDQ SHQDPEDKDQ NHWHEDODQ FKRUG OXDU VDMD PHPEHULNDQ SHQDPEDKDQ NDSDVLWDV \DQJ FXNXS VLJQLILNDQ WHUKDGDS NDSDVLWDV VDPEXQJDQ WXEXODU GLJURXW *UDGLHQ NHQDLNDQ NDSDVLWDV VHGLNLW PHQXUXQ GHQJDQ EHUWDPEDKQ\D NHWHEDODQ FKRUG OXDU GDQ NDSDVLWDV KDPSLU PHUXSDNDQ IXQJVL OLQLHU WHUKDGDS NHWHEDODQ HIHNWLI +DO LQL FXNXS VHVXDL GHQJDQ IRUPXODVL GDODP SHUDWXUDQ$3,53$:6'

'DIWDU3XVWDND

  • $%$486 ³$%$486&$( 8VHU V 0DQXDO´2QOLQH'RFXPHQWDWLRQ+HOS'DVVDXOW 6\VWqPHV
  • $3,53$-:6' $3,5HFRPPHQGHG3UDFWLFH IRU 3ODQQLQJ 'HVLJQLQJ DQG &RQVWUXFWLRQ )L[HG2IIVKRUH3ODWIRUP:RUNLQJ6WUHVV'HVLJQ $PHULFDQ3HWUROHXP,QVWLWXWH$3, 86$
  • *RPHV 1 9 /52 GH /LPDD 3&* GD 6 9HOODVFRD $7 GD 6LOYDD 0& 5RGULJXHVD /) &RVWD-1HYHVF ³([SHULPHQWDO DQG QXPHULFDO LQYHVWLJDWLRQ RI 6+6 WUXVV 7-MRLQWV UHLQIRUFHG ZLWK VLGHZDOO SODWHV´ - RI 7KLQ- :DOOHG6WUXFWXUHV
  • 0HOHN 3 * +XVVHLQ 0 DQG *DDZDQ 6 ³&RQILQLQJ7-MRLQWVE\DGGLQJWZRRXWHUKROORZ ULQJIODQJHVZHOGHGWRDGGLWLRQDOKROORZFLUFXODU SLSH´ &DQDGLDQ -RXUQDO RI &LYLO (QJLQHHULQJ -
  • 1RUVRN6WDQGDUG1- 5HY2FWREHU 'HVLJQ RIVWHHOVWUXFWXUHV6WDQGDUG1RUZD\
  • 3HFNQROG ' $ 3DUN -% DQG .RSSHQKRHIHU .& ³8OWLPDWH 6WUHQJWK RI *DS . 7XEXODU -RLQW ZLWK &KRUG 3UHORDGV´ LQ 3URFHHGLQJV RV 20$(¶ WK ,QWHUQDWLRQDO &RQIHUHQFH RQ 2IIVKRUH0HFKDQLFVDQG$UFWLF(QJLQHHULQJ5LR GH-HQHLUR%UD]LO
  • 6KHQ: DQG&KRR< 6 ³6WUHVV )DFWRU IRU D 7XEXODU 7-MRLQW ZLWK *URXWHG &KRUG´ - (QJLQHHULQJ6WUXFWXUH-
  • 6KHQJ]KL 6 <RQJER 6 ³6WDWLF 6WUHQJWK RI 7XEXODU 7-MRLQW ZLWK 5HLQIRUFHG &KRUG 8QGHU ,Q-SODQH %HQGLQJ /RDG´ 7KH 2SHQ 2FHDQ (QJLQHHULQJ-RXUQDO-
  • 6KXELQ +( <RQJER 6 DQG +RQJ\DQ = ³6WDWLF 6WUHQJWK RI &LUFXODU 7XEXODU 7-MRLQWV ZLWK ,QQHU 'RXEOHU 3ODWH 5HLQIRUFHPHQW 6XEMHFWHG WR $[LDO &RPSUHVVLRQ´ 7KH 2SHQ 2FHDQ (QJLQHHULQJ-RXUQDO-
  • 6XDUMDQD 0 .XUQLD 0 ³3HQJXMLDQ 3HUXPXVDQ &RGH $3, $PHULFDQ 3HWUROHXP ,QVWLWXWH XQWXN -RLQW %DMD 7XEXODU WLGDN 'LJURXW GDQ 'LJURXW GHQJDQ 0HWRGD (OHPHQ +LQJJD´ -XUQDO 7HNQLN 6LSLO ,QVWLWXW 7HNQORJL %DQGXQJ -
  • 6ZHQVVRQ.'<XUD-$ 8OWLPDWH6WUHQJWK RI 'RXEOH-7HH 7XEXODU -RLQW ,QWHUDFWLRQ (IIHFWV 30)6(/ 5HSRUW 1R - 7KH 8QLYHUVLW\RI7H[DV$XVWLQ86$
  • 7KRUHQIHOGW ( 7RPDV]HZLF] $ GDQ -HQVHQ - ³0HFKDQLFDOSURSHUWLHVRIKLJK-VWUHQJWK FRQFUHWH DQG DSSOLFDWLRQ LQ GHVLJQ´ 3URFHHGLQJV RI 6\PSRVLXP RQ 8WLOL]DWLRQ RI +LJK-6WUHQJWK &RQFUHWH 7DSLU 7URQGKHLP 1RUZD\
  • 9DQ GHU 9HJWH *- 0DNLQR < DQG :DUGHLQHU ³7KH (IIHFW RI &KRUG 3UH-ORDG RQ 7KH 6WDWLF6WUHQJWKRI8QLSODQDU7XEXODU.--RLQWV´ 3URFHHGLQJVRI7KH7ZHOIWK 2IIVKRUHDQG3RODU (QJLQHHULQJ&RQIHUHQFH.LWDN\XVKX-HSDQJ
  • :HL 6 %HKDYLRXU RI *URXW ,QILOOHG 6WHHO 7XEXODU 0HPEHUV $QG -RLQWV 3K ' 7KHVLV 1DWLRQDO8QLYHUVLW\RI6LQJDSRUH6LQJDSRUH
  • <XUD $ =HWWOHPR\HU 1 $ DQG (GZDUGV , ) ³8OWLPDWH &DSDFLW\ (TXDWLRQV IRU 7XEXODU -RLQWV´ 2IIVKRUH 7HFKQRORJ\ &RQIHUHQFH+RXVWRQ7H[DV86$

Research Intelligence

Data from OpenAlex ↗

Metrics

0.00
FWCIfield-weighted
10th
Percentilevs same year + field
Article
Work type
Open Access

Institution Network

References

  1. ABAQUS (2011), "ABAQUS/CAE 6.11 User
  2. API RP 2A-WSD (2007), API Recommended Practice for Planning, Designing, and Construction Fixed Offshore Platform Working Stress Design, American Petroleum Institute (API), USA.
  3. Gomes, N. V., L.R.O. de Limaa, P.C.G. da S. Vellascoa, A.T. da Silvaa, M.C. Rodriguesa, L.F. Costa-Nevesc, (2019), "Experimental and numerical investigation of SHS truss T-joints reinforced with sidewall plates" , J. of Thin-Walled Structures, 145: 106404
  4. Melek, P. G., Hussein, M. and Gaawan, S. (2017), "Confining T-joints by adding two outer hollow ring flanges welded to additional hollow circular pipe" , Canadian Journal of Civil Engineering, 44(10): 783-801
  5. Norsok Standard N-004 (Rev. October 2004) : Design of steel structures, Standard Norway.
  6. Pecknold, D. A, Park, J.B., and Koppenhoefer, K.C., (2001), "Ultimate Strength of Gap K Tubular Joint with Chord Preloads" , in Proceedings os OMAE
  7. Shen, W. and Choo, Y. S. (2012), "Stress Factor for a Tubular T-joint with Grouted Chord" , J. Engineering Structure, 35:37-47
  8. Shengzhi, S., Yongbo, S., (2011), "Static Strength of Tubular T-joint with Reinforced Chord Under In-plane Bending Load" , The Open Ocean Engineering Journal, 4: 65-70
  9. Shubin, H.E., Yongbo, S., and Hongyan, Z., (2013), "Static Strength of Circular Tubular T-joints with Inner Doubler Plate Reinforcement Subjected to Axial Compression" , The Open Ocean Engineering Journal. 6: 1-7
  10. Suarjana, M., Kurnia, M.,(2013), "Pengujian Perumusan Code API (American Petroleum Institute) untuk Joint Baja Tubular tidak Digrout dan Digrout dengan Metoda Elemen Hingga" , Jurnal Teknik Sipil, Institut Teknlogi Bandung, 20(3): 195-206
  11. Swensson, K. D., Yura J. A., (1987), Ultimate Strength of Double-Tee Tubular Joint: Interaction Effects, PMFSEL Report No. 87-9, The University of Texas, Austin, USA.
  12. Thorenfeldt, E. Tomaszewicz, A. dan Jensen J. J., (1987), "Mechanical properties of high-strength concrete and application in design," Proceedings of Symposium on Utilization of High-Strength Concrete, Tapir, Trondheim, Norway.
  13. Van der Vegte, G.J., Makino, Y., and Wardeiner, J., (2002), "The Effect of Chord Pre-load on The Static Strength of Uniplanar Tubular K-Joints" , Proceedings of The Twelfth Offshore and Polar Engineering Conference. Kitakyushu, Jepang.
  14. Wei, S. (2011), Behaviour of Grout Infilled Steel Tubular Members And Joints, Ph. D. Thesis, National University of Singapore, Singapore.
  15. Yura, J. A., Zettlemoyer, N. A., and Edwards, I. F. (1980). "Ultimate Capacity Equations for Tubular Joints" . Offshore Technology Conference. Houston, Texas, USA.